LABORATORIUM MEKENIKA TANAH

JURUSAN TEKNIK SIPIL


POLITEKNIK NEGERI LHOKSEUMAWE

SUMMARY DESIGN MIX FORMULA


DMF AC - BC
I. KOMPOSISI CAMPURAN AGGREGAT COLD BIN

MATERIAL PROPORSI ( % ) BUKAAN COLD BIN ( cm )

COARSE AGGREGATE COLD BIN I 30.0 % 28.2 % 4.4 cm

MEDIUM AGGREGATE COLD BIN II 30.0 % 28.2 % 7.2 cm

DUST STONE COLD BIN III 30.0 % 28.2 % 5.4 cm

SAND COLD BIN IV 10.0 % 9.4 % 4.4 cm

ASPHALT 5.95 %

TOTAL 100.0 % 100.0 %

II. MARSHALL PROPERTIES

MIX PROPERTIES TEST RESULT REQUIREMENT

PENYERAPAN KADAR ASPAL 2.40 Max. 1.2

RONGGA DALAM CAMPURAN % 5.3 3.5 - 5.5

RONGGA DALAM AGGREGAT % 13.1 Min. 14

RONGGA TERISI ASPAL % 81.5 Min. 63

STABILITAS MARSHALL kg 941 Min. 800

KELELEHAN mm 3.2 Min. 3

MARSHALL QUOTIENT kg/mm 291.5 Min. 200

STABILITAS MARSHALL SISA % 87.1 Min. 85

RONGGA DALAM CAMPURAN (REFUSAL) % - Min. 2.5

BERAT ISI 2.325

TEMPERATUR MIXING c 150 Max. 155

III. GRADASI AGGREGATE GABUNGAN


Inc. 1" 3 / 4" 1 / 2" 3 / 8" #4 #8 # 16 # 30 # 50 #100 # 200
UKURAN SARINGAN
mm. 25.4 19 12.7 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075

TOTAL CAMP. 0% 100.0 99.8 79.5 71.3 48.2 34.9 28.4 23.7 18.0 6.5 0.8

MINIMUM 100.0 90 74 64 47 34.6 28.3 20.7 13.7 4 4


SPECT' GRAD.
MAXIMUM 100.0 100 90 82 64 49.0 38 28 20 13 8

FULLER 100.0 87.8 73.2 64.2 47.0 34.3 25.1 18.5 13.6 9.9 7.3
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Aggregat
Wt. Sample : 2996.9 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.0 100.0 25

3/4" 19.1 19 0.6 99.4

1/2" 1913.7 1933 64.5 35.5

3/8" 639.2 2572 85.8 14.2

#4 374.8 2947 98.3 1.7

#8 45 2992 99.8 0.2

# 16 0.3 2992 99.8 0.2

# 30 0.3 2992 99.8 0.2

# 50 0.1 2993 99.9 0.1

#100 0.8 2993 99.9 0.1

# 200 3.6 2997 100.0 0.0


TO TAL PASSING ( % )

GRADING CHART

100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0 #200 #100 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"
SIEVE SIZE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC


NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Aggregat 3/8"
Wt. Sample : 2950.5 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.00 100.00 11

3/4" 0 0 0.00 100.00

1/2" 117.1 117 3.97 96.03

3/8" 173.40 290.50 9.85 90.15

#4 1898.10 2188.60 74.18 25.82

#8 384.40 2573.00 87.21 12.79

# 16 77.60 2650.60 89.84 10.16

# 30 47.00 2697.60 91.43 8.57

# 50 41.10 2738.70 92.82 7.18

# 100 83.30 2822.00 95.64 4.36

# 200 128.50 2867.20 97.18 2.82


TO TAL PASSING ( % )

GRADING CHART

100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0 #200 #100 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"
SIEVE SIZE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC


NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Dust Stone
Wt. Sample : 2827.9 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.0 100.0 321

3/4" 0 0 0.0 100.0 2827.9

1/2" 0 0 0.0 100.0

3/8" 0 0 0.0 100.0

#4 8.7 9 0.3 99.7

#8 834.6 843 29.8 70.2

# 16 521.9 1365 48.3 51.7

# 30 305.4 1671 59.1 40.9

# 50 255.1 1926 68.1 31.9

# 100 370.8 2297 81.2 18.8

# 200 531.4 2828 100.0 0.0


TO TAL PASSING ( % )

GRADING CHART

100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0 #200 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"


SIEVE SIZE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC


NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Natural Sand
Wt. Sample : 8175 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.0 100.0 375

3/4" 0 0 0.0 100.0 8175.00

1/2" 0 0 0.0 100.0

3/8" 0 0 0.0 100.0

#4 0 0 0.0 100.0

#8 4.00 4.00 0.05 99.95

# 16 210.00 214.00 2.62 97.38

# 30 749.00 963.00 11.78 88.22

# 50 2111.00 3074.00 37.60 62.40

#100 2898.00 5972.00 73.05 26.95

# 200 2203.00 8175.00 100.00 0.00


TO TAL PASS ING ( % )

GRADING CHART
100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0
#200 #100 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"
0.0
SIEVE SIZE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC

ANALYST AGGREGATE SURFACE AREA


ASTM AGGREGATE GRADING AGGREGATE
COMBINED AGGREGATE GRADING
SIEVE CA MA DS SA SURFACE

SIZE a b c d I II III IV V VI VII VIII IX X XI XII XIII XIV XV XVI XVII XVIII XIX XX XXI FACTOR

1 1/2"

1" 100 100 100 100 100.0

3/4" 99.362675 100 100 100 99.8 100 100 100 100 100 100 100 100 100 100 100 100 100 100
1 x 0.41
1/2" 35.50669 96.031181 100 100 79.5 89.1 85.6 92.6 89.1 85.5 92.6 89.0 85.5 89.0 89.0 89.0 89.0 89.0 89.0

3/8" 14.177984 90.154211 100 100 71.3 85.1 80.2 89.7 84.9 80.1 89.6 84.8 80.0 84.8 84.8 84.8 84.8 84.8 84.8

#4 1.7 25.822742 99.692351 100 48.2 76.2 69.4 81.9 75.1 68.4 80.7 74.1 67.4 73.9 73.9 73.9 73.9 73.9 73.9 x 0.41

#8 0.1701758 12.794442 70.179285 99.95107 34.9 67.4 60.9 68.7 62.7 56.7 63.7 58.3 52.6 57.9 57.9 57.9 57.9 57.9 57.9 x 0.82

# 16 0.2 10.2 51.723894 97.382263 28.4 61.3 55.4 60.1 54.8 49.6 53.2 48.6 43.9 48.3 48.3 48.3 48.3 48.3 48.3 x 1.64

# 30 0.1501552 8.5714286 40.924361 88.220183 23.7 54.0 48.8 52.0 47.5 42.9 45.1 41.2 37.2 40.8 40.8 40.8 40.8 40.8 40.8 x 2.87

# 50 0.1468184 7.2 31.9 62.397554 18.0 39.1 35.3 38.1 34.8 31.5 33.5 30.7 27.7 30.4 30.4 30.4 30.4 30.4 30.4 x 6.14

# 100 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 x 12.29

# 200 0.1201241 2.8 18.8 0.0 6.5 4.9 4.5 7.7 7.1 6.5 10.1 9.2 8.4 9.3 9.3 9.3 9.3 9.3 9.3 x 32.77

Agg. Blend a. Coarse Agg. ( CA ) 30.0 16.2 21.6 10.8 16.2 21.6 10.8 16.2 21.6 16.2 16.2 16.2 16.2 16.2 16.2

ratio b. Medium Agg. ( MA ) 30.0 10.5 12.5 9.9 11.9 13.8 11.5 13.2 15.1 13.5 13.5 13.5 13.5 13.5 13.5

( % by wt. c. Dust Stone ( DS ) 30.0 24.4 21.9 39.6 35.9 32.3 51.8 47.1 42.2 47.2 47.2 47.2 47.2 47.2 47.2

of total agg. d. Sand Agg. ( SA ) 10.0 48.9 43.9 39.6 35.9 32.3 25.9 23.5 21.1 23.0 23.0 23.0 23.0 23.0 23.0

TOTAL AGGREGATE SURFACE AREA 5.3 7.8 7.1 8.7 8.0 7.3 8.8 8.1 7.4 8.1 8.1 8.1 8.1 8.1 8.1
1:2 1:1 2:1 2:1

Remark's :
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL
LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC WC

KOMPOSISI JOB MIX FORMULA

UKURAN SARINGAN

DATA MATERIAL KOMPOSISI Inc. 1" 3 / 4" 1 / 2" 3 / 8" #4 #8 # 16 # 30 # 50 #100 # 200

mm. 25.4 19 12.7 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075
AGG. 1" 30% 100.0 99.4 35.5 14.2 1.7 0.2 0.2 0.2 0.1 0.1 0.0
% PASS. SIEVE

AGG. 3/8" 30% 100.0 100.0 96.0 90.2 25.8 12.8 10.2 8.6 7.2 2.8 2.8
DUST STONE 30% 100.0 100.0 100.0 100.0 99.7 70.2 51.7 40.9 31.9 18.8 0.0
SAND 10% 100.0 100.0 100.0 100.0 100.0 100.0 97.4 88.2 62.4 0.0 0.0
TOTAL CAMP. 100% 100.0 99.8 79.5 71.3 48.2 34.9 28.4 23.7 18.0 6.5 0.8
MINIMUM 100.0 90 74 64 47 34.6 28.3 20.7 13.7 4 4
SPECT' GRAD.
MAXIMUM 100.0 100 90 82 64 49.0 38 28 20 13 8
FULLER 100.0 87.8 73.2 64.2 47.0 34.3 25.1 18.5 13.6 9.9 7.3

Perkiraan Kadar Aspal Optimum Pb = 0,035 (69,2%) + 0,045 (26,1%) + 0,18 (4,7) + 1
0.035 65.1 0.045 28.4 0.18 6.5 1
Pb = 5.7 %

% Kadar Aspal untuk Benda Uji = 4.2 4.7 5.2 5.7 6.2 6.7 7.2

GRADING CHART

Hasil Gradasi
Batas Spec Fuller
100 Gabungan
TOTAL % PASSING

90

80

70

60

50

40

30

20

10

0 #200 #100 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"

SIEVE SIZE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL


LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

SPECIFIC GRAVITY AND ABSORPTION TEST OF COARSE AGGREGATE


SNI 03-1969-1990
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Aggregat 1"

SIZE PARTIKEL

RUN NO.

1 WEIGHT OF ( SSDC + DISH) ( gr ) 1016.40 1016.40

2 WEIGHT OF DISH ( gr ) 0.00 0.00

3 WEIGHT OF SSDC ( gr ) 1-2 1016.40 1016.40

WEIGHT OF (WIRE BASKET + SSDC)


4 ( gr ) 625.14 625.14
IN WATER

5 WEIGHT OF WIRE BASKET IN WATER ( gr ) 0.00 0.00

6 WEIGHT OF SSDC IN WATER ( gr ) 4-5 625.14 625.14

7 SPGR OF SSDC ( gr ) 3 / (3 - 6) 2.60 2.60

AVERAGE 2.60

8 WEIGHT OVEN DRY SAMPLE 1000.70 1000.70

9 BULK SPGR ( gr ) 8 / (3 - 6) 2.56 2.56

AVERAGE 2.56

10 VOLUME OF WATER 3-8 15.70 15.70

11 APPARENT SPGR ( gr ) 8 / (8 - 6) 2.66 2.66

AVERAGE 2.66

12 ABSORPTION PERCENT (%) (10/8) x 100 1.57 1.57

AVERAGE 1.57
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL


LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

SPECIFIC GRAVITY AND ABSORPTION TEST OF COARSE AGGREGATE


SNI 03-1969-1990
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Aggregat 3/8"

SIZE PARTIKEL

RUN NO. I II

1 WEIGHT OF ( SSDC + DISH) ( gr ) 509.40 509.40

2 WEIGHT OF DISH ( gr ) 0.00 0.00

3 WEIGHT OF SSDC ( gr ) 1-2 509.40 509.40

WEIGHT OF (WIRE BASKET + SSDC)


4 ( gr ) 313.83 313.83
IN WATER

5 WEIGHT OF WIRE BASKET IN WATER ( gr ) 0.00 0.00

6 WEIGHT OF SSDC IN WATER ( gr ) 4-5 313.83 313.83

7 SPGR OF SSDC ( gr ) 3 / (3 - 6) 2.60 2.60

AVERAGE 2.60

8 WEIGHT OVEN DRY SAMPLE 500.67 500.67

9 BULK SPGR ( gr ) 8 / (3 - 6) 2.56 2.56

AVERAGE 2.56

10 VOLUME OF WATER 3-8 8.73 8.73

11 APPARENT SPGR ( gr ) 8 / (8 - 6) 2.68 2.68

AVERAGE 2.68

12 ABSORPTION PERCENT (%) (10/8) x 100 1.74 1.74

AVERAGE 1.74
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SPECIFIC GRAVITY AND ABSORPTION TEST OF FINE AGGREGATE


SNI 03-1970-1990
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Dust Stone

RUN NO.

NO. OF FLASK

A WEIGHT OF SAMPLE ( S.S.D) ( gr ) 500.0 500.0

B WEIGHT OF FLASK + WATER ( gr ) 1305.5 1293.5

C WEIGHT OF FLASK + WATER + SAMPLE ( gr ) 1617.8 1605.0

D WEIGHT OF DRY SAMPLE ( gr ) 465.7 467.0

1 S.S.D SPGR ( gr ) A/(A+B-C) 2.664 2.653

AVERAGE 2.658

2 BULK SPGR ( gr ) D/(A+B-C) 2.481 2.477

AVERAGE 2.479

3 APPARENT SPGR ( gr ) D/(B+D-C) 3.036 3.003

AVERAGE 3.020

4 ABSORPTION (%) (A-D)/Dx100 7.365 7.066

AVERAGE 7.216
REGATE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

SPECIFIC GRAVITY AND ABSORPTION TEST OF FINE AGGREGATE


SNI 03-1970-1990
Tanggal Pengujian : 23 Juli - 07 Agustus 2015
Material : Dust Stone

RUN NO.

NO. OF FLASK

A WEIGHT OF SAMPLE ( S.S.D) ( gr ) 500.0 500.0

B WEIGHT OF FLASK + WATER ( gr ) 1470.4 1462.2

C WEIGHT OF FLASK + WATER + SAMPLE ( gr ) 1776.5 1768.2

D WEIGHT OF DRY SAMPLE ( gr ) 487.2 487.4

1 S.S.D SPGR ( gr ) A/(A+B-C) 2.579 2.577

AVERAGE 2.578

2 BULK SPGR ( gr ) D/(A+B-C) 2.513 2.512

AVERAGE 2.513

3 APPARENT SPGR ( gr ) D/(B+D-C) 2.690 2.687

AVERAGE 2.689

4 ABSORPTION (%) (A-D)/Dx100 2.627 2.585

AVERAGE 2.606
REGATE
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

ANALISA VOLUMEMERIK

Specific Grafity (kg/cm3)


No Material Percentage (P) Absorbsi (%) Formula
Bulk (Gblk) Apparent (Gap)

1 Agg. 1" 30.0 2.558 2.665 1.569

2 Agg. 3/8" 30.0 2.560 2.680 1.744

3 Dust Stone 30.0 2.479 3.020 7.216

4 Natural Sand 10.0 2.513 2.689 2.606

5 Gs Max of Mixture (Gmm) = 2.491 gr/cm3 AASHTO T 209 pada kadar aspal opt. perkiraan

6 Gs Eff of total Aggregate (Gse) = 2.663 gr/cm3 (100)/(2)/(Gsap)+Gsb/2

7 Gs Bulk of total Aggregate (Gsb) = 2.517 gr/cm3 100/((P1/Gblk1)+(P2/Gblk2)

8 Gs Apparent of tota Aggregate (Gsap) = 2.810 gr/cm3 100/((P1/Gap1)+(P2/Gap2)

9 Gs Bitument (Gb) = 1.100 gr/cm3 AASHTO T 228

10 Absorb. Bitument Content (Pba) = 2.4 % 100*(Gse-Gsb)/(Gsb*Gse)*Gb

11 Opt. Bitument Cont. (estimate) (Pb) = 5.7 % 0.035(%CA)+0.045(%FA)+0.18(%FF)+C

12 Effective Bitument (Pbe) = 3.4 % Pb-(Pba*100-Pb)/100

13 Agg. Surface Area (Asa) = 5.3

14 Bitumen Film Thickness (Bft) = 7.8 micron 1000*(Pb-Pba)/(Asa*(Gb*(100-Pb)))


LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC
NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL
LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

GRAFIK DATA MARSHALL


Kepadatan (gr/cm)

Kadar Aspal >< Stabilitas


Kadar Aspal >< Kepadatan
1800
2.38

Satabilitas (kg)
1600
2.36

1400
2.34

2.32 1200

2.30 1000

2.28 800

2.26 600

3.7 4.2 4.7 5.2 5.7 6.2 6.7 3.70 4.20 4.70 5.20 5.70 6.20 6.70
Kadar Aspal (%)
Kadar Aspal (%)

Kadar Aspal >< Kelelehan Kadar Aspal >< Marshall quotien


5.0 500.00
Flow (%)

M Q (%)

4.0 400.00

3.0 300.00

2.0 200.00

1.0 100.00

0.0 0.00

3.70 4.20 4.70 5.20 5.70 6.20 6.70 3.70 4.20 4.70 5.20 5.70 6.20 6.70
Kadar Aspal (%) Kadar Aspal (%)

Kadar Aspal >< Rongga thd. Campuran (V I M) Kadar Aspal >< Rongga Diantara Agg. (V M A)
(%)

8.00 17.00
.V M A (%)

7.00
VIM

16.00
6.00

15.00
5.00

4.00
14.00

3.00
13.00
2.00

1.00 12.00

3.70 4.20 4.70 5.20 5.70 6.20 6.70 3.70 4.20 4.70 5.20 5.70 6.20 6.70
Kadar Aspal (%) Kadar Aspal (%)

Kadar Aspal >< Rongga terisi aspal(V F B) Kadar Aspal >< V I M at P R D


100.00 8
MARSHALL 75 X 2
V I M (%)
(%)

7
80.00
VFB

60.00
5

40.00 4

3
20.00
PRD 400 X 2
2

0.00 1

3.70 4.20 4.70 5.20 5.70 6.20 6.70 3.70 4.20 4.70 5.20 5.70 6.20 6.70
Kadar Aspal (%) Kadar Aspal (%)
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA PAKET : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KONTRAKTOR : -

KONSTRUKSI : AC - BC

BAR CHART

RENTANG KADAR ASPAL TOTAL


SIFAT - SIFAT CAMPURAN

3.70 4.20 4.70 5.20 5.70 6.20 6.70 7.50 8.00

RONGGA DALAM AGGREGAT (VMA)

RONGGA TERISI ASPAL (VFB)

STABILITAS MARSHALL

KELELEHAN

MARSHALL QUOTIENT

RONGGA DALAM CAMPURAN DAN

RONGGA DALAM CAMPURAN (REFUSAL)

KADAR ASPAL OPTIMUM = 5,95 %

5.95
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL

LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE

KELAS : -

KONSTRUKSI : AC - BC

BERAT JENIS MAKSIMUM CAMPURAN BERASPAL


SNI 03-6893-2002

NO URAIAN I II

A BERAT BENDA UJI KERING 5525 5648

B BERAT WADAH DALAM AIR 0 0

C BERAT BENDA UJI DALAM AIR 3305 3382

D BERAT JENIS A / A- C 2.489 2.492

F AVERAGE 2.491
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC
NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL
LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 2.578 BJ. EFFECTIVE AGGREGATE ( U ) 2.598 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 4.73 4.96 1157 567.00 1100.69 534 2.168 88 1223 1174 3.2 367.0
2 1183 587.60 1086.40 499 2.372 98 1362 1308 3.2 408.7
3 1175 574.00 1080.88 507 2.318 87 1209 1161 3.2 362.8
Avg 4.73 4.96 513.123 2.286 2.441 15.7 6.3 77.9 1214 3.2 379.5

1 5.23 5.52 1151 609.60 1098.50 489 2.354 115 1599 1535 3.77 407.0
2 1143 598.10 1099.30 501 2.281 115 1599 1535 3.6 426.3
3 1135 592.30 1097.70 505 2.246 99 1376 1321 3.7 357.0
Avg 5.23 5.52 498.500 2.294 2.425 15.9 5.4 78.6 1463 3.7 396.8

1 5.73 6.08 1122 611.20 1099.33 488 2.299 120 1668 1601 3.69 434.0
2 1125 610.50 1093.18 483 2.331 120 1668 1601 3.8 421.4
3 1122 602.70 1092.55 490 2.290 123 1710 1641 4.2 390.8
Avg 5.73 6.08 486.887 2.307 2.410 16.0 4.3 79.7 1615 3.9 415.4

1 6.23 6.64 1124 601.50 1087.00 486 2.315 118 1640 1575 4.71 334.3

2 1123 607.60 1089.00 481 2.333 122 1696 1628 4.3 378.6

3 1145 602.20 1099.00 497 2.305 114 1585 1521 3.6 422.6

Avg 6.23 6.64 487.900 2.318 2.395 16.1 3.2 80.7 1575 4.2 378.5

1 6.73 7.22 1118 602.60 1080.70 478 2.338 117 1626 1561 4.57 341.6

2 1116 611.30 1090.20 479 2.330 79 1098 1054 3.9 270.3

3 1113 609.80 1093.30 484 2.302 113 1571 1508 4.5 335.1

Avg 6.73 7.22 480.167 2.324 2.380 16.4 2.4 81.3 1374 4.3 315.7
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC
NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL
LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 2.517 BJ. EFFECTIVE AGGREGATE ( U ) 2.663 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 6.00 6.38 1064.2 588.4 1051.80 463 2.297 70 973 934 3.5 266.9
2 1063.4 594.0 1050.50 457 2.329 75 1043 1001 3.2 312.8
3 1062.0 592.4 1052.62 460 2.308 77 1070 1027 3.1 331.4
Avg 6.00 6.38 460.030 2.311 2.454 14.0 5.8 80.1 987 3.3 303.7

1 6.50 6.95 1053.0 593.6 1047.30 454 2.321 80 1112 1068 3.5 305.0
2 1055.4 590.7 1050.50 460 2.295 81 1126 1081 3.6 300.2
3 1052.0 592.2 1048.90 457 2.303 81 1119 1074 4 302.6
Avg 6.50 6.95 456.750 2.306 2.438 14.7 5.4 79.9 1074 3.6 302.6

1 7.00 7.53 1046.0 604.2 1052.50 448 2.333 70 973 934 3.6 259.5
2 1044.0 596.7 1057.30 461 2.267 73 1015 974 3.4 286.5
3 1045.0 600.5 1054.90 454 2.299 72 994 954 4 272.6
Avg 7.00 7.53 454.450 2.300 2.422 15.5 5.1 79.4 954 3.5 272.9
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC / AC - WC

NAMA KEGIATAN :
LOKASI :
KELAS :
KONSTRUKSI : Laston AC - WC/ AC - BC
MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 2.517 BJ. EFFECTIVE AGGREGATE ( U ) 2.663 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 7.00 7.53 1032 590 1027.3 438 2.357 68 945 907 3.3 275.0
2 1028 602 1047.3 445 2.309 66 917 881 3.5 251.6
3 1030 596 1037 442 2.333 67 931 894 3.4 263.0
Avg 7.00 7.53 441.500 2.333 2.422 13.8 3.7 82.5 894 3.4 263.2
LABORATORIUM MEKENIKA TANAH
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA KEGIATAN : PRAKTIKUM LABORATORIUM ASPAL
LOKASI : LABORATORIUM JALAN RAYA JURUSAN TEKNIK SIPIL POLITEKNIK NEGERI LHOKSEUMAWE
KELAS : -
KONSTRUKSI : AC - BC

MARSHALL TEST (STABILITAS SISA)


RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 2.517 BJ. EFFECTIVE AGGREGATE ( U ) 2.663 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 5.95 6.33 1256 734 1268 534 2.351 70 980 941 3.4 276.7
2 1242 723 1272 549 2.263 68 952 914 3.0 304.6
3 1256 733 1265 532 2.361 72 1008 968 3.3 293.2
Avg 5.95 6.33 538.333 2.325 2.456 13.1 5.3 81.5 941 3.2 291.5
PERENDAMAN 24 JAM PADA SUHU 60C
1 5.95 6.33 1241 722 1273 551 2.252 65 910 874 2.7 323.6
2 1251 728 1262 534 2.343 60 840 806 3.0 268.8
3 1267 741 1275 534 2.372 58 812 780 2.5 311.8
Avg 5.95 6.33 539.667 2.323 2.456 13.2 5.4 81.4 820 2.7 301.4

STABILITAS SISA SETELAH PERENDAMAN 24 JAM PADA SUHU 60C Min. 85% = 820 / 941 x 100 = 87.1 %
PERHITUNGAN KOMPOSISI CAMPURAN
BERAT MASING - MASING AGGREGAT DALAM SATUAN GRAM UNTUK 1 (SATU) BUAH BENDA UJI
CA = 30.0%
MA = 30.0%
DUST = 30.0%
SAND = 10.0%
ASPAL PB = 5.7%

PB 4.23 4.73 5.23


BERAT TOT. TBENDA UJI 1200 1200 1200
CAMPURAN % PROPORSI INDV. Gram Komul. Gram % PROPORSI INDV. Gram Komul. Gram % PROPORSI INDV. Gram Komul. Gram
COARSE AGGREGAT 25 23.94 287.31 287.31 25 23.44 281.31 281.31 25 22.94 275.31 275.31
MEDIUM AGGREGAT 30 28.731 344.77 632.08 30 28.731 344.77 626.08 30 28.731 344.77 620.08
DUST 25 23.943 287.31 919.40 25 23.943 287.31 913.40 25 23.943 287.31 907.40
SAND 20 19.154 229.85 1149.24 20 19.154 229.85 1143.24 20 19.154 229.85 1137.24
ASPAL 4.23 50.76 1200.00 4.73 56.76 1200.00 5.23 62.76 1200.00
TOTAL 100 100.00 1200.00 100 100.00 1200.00 100 100.00 1200.00

PB 5.73
BERAT TOT. TBENDA UJI 1200
CAMPURAN % PROPORSI INDV. Gram Komul. Gram
COARSE AGGREGAT 25 22.44 269.31 269.31
MEDIUM AGGREGAT 30 28.731 344.77 614.08
DUST 25 23.943 287.31 901.40
SAND 20 19.154 229.85 1131.24
ASPAL 5.73 68.76 1200.00
TOTAL 100 100.00 1200.00

PB 6.23 6.73 7.23


BERAT TOT. TBENDA UJI 1200 1200 1200
CAMPURAN % PROPORSI INDV. Gram Komul. Gram % PROPORSI INDV. Gram Komul. Gram % PROPORSI INDV. Gram Komul. Gram
COARSE AGGREGAT 25 21.94 263.31 263.31 25 21.44 257.31 257.31 25 20.94 251.31 251.31
MEDIUM AGGREGAT 30 28.731 344.77 608.08 30 28.731 344.77 602.08 30 28.731 344.77 596.08
DUST 25 23.943 287.31 895.40 25 23.943 287.31 889.40 25 23.943 287.31 883.40
SAND 20 19.154 229.85 1125.24 20 19.154 229.85 1119.24 20 19.154 229.85 1113.24
ASPAL 6.23 74.76 1200.00 6.73 80.76 1200.00 7.23 86.76 1200.00
TOTAL 100 100.00 1200.00 100 100.00 1200.00 100 100.00 1200.00
DIAGRAM BERAT

Berat Benda = 1100 gr Jumlah Total 35%


Pb = 5.6 1038.4 35%
Berat Aspal Pb = 61.6 61.6 1038.4 10%
Split = 311.5 934.56 519.2 20%
Scren = 311.5 934.56 519.2
Dust = 311.5 934.56
Sand = 103.8 311.52
Jumlah = 1100 3177

Berat Benda = 1100


Pb = 5.1
Berat Aspal Pb = 56.1 56.1
Split = 365.4 1096.095
Scren = 365.4 1096.095
Dust = 104.4 313.17
Sand = 208.8 626.34
Jumlah = 1100 3188

Berat Benda = 1100


Pb = 6.1
Berat Aspal Pb = 67.1 67.1
Split = 361.515 1084.545
Scren = 361.515 1084.545
Dust = 103.29 309.87
Sand = 206.58 619.74
Jumlah = 1100 3166
Ket :
Pb = 0.1 dari 5.6 %