Anda di halaman 1dari 10

No.

Formulir

FORMULIR Terbitan/Revisi

Tanggal Revisi

PERENCANAAN
LAB.PENGUJIAN BALAI Halaman 1 dari 1
LITBANG PERKERASAN JALAN PENGGABUNGAN AGREGAT

1. No. Order/Contoh : PKL SMKN 1 MAUMERE


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING
3. Jenis Pekerjaan
4. Diterima tanggal :
5. Di uji tanggal : 25 MARET 2019
6. Metode uji : -
7. Hasil pengujian :

URAIAN
Inch 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 #100 #200
mm 19.0 12.5 9.5 4.75 2.36 1.18 0.600 0.300 0.150 0.075
DATA GRADASI
Agregat KASAR 100.0 12.6 2.7 1.1 0.9 0.8 0.6 0.6 0.6 0.5
Agregat SEDANG 100.0 100.0 97.2 26.3 6.4 5.3 4.6 4.2 3.2 2.1
AGREGAT HALUS 100.0 100.0 100.0 96.3 69.1 44.3 28.8 18.6 12.2 8.8

KOMBINASI AGREGAT
Agregat KASAR 11.0% 11.0 1.4 0.3 0.1 0.1 0.1 0.1 0.1 0.1 0.1
Agregat SEDANG 34.0% 34.0 34.0 33.0 8.9 2.2 1.8 1.6 1.4 1.1 0.7
AGREGAT HALUS 55.0% 55.0 55.0 55.0 53.0 38.0 24.3 15.8 10.2 6.7 4.8

Gradasi gabungan 100.0 100.0 90.4 88.3 62.0 40.3 26.2 17.5 11.7 7.8 5.6
Gradasi Laston AC BASE
Maks. 100.0 100.0 90.0 69.0 53.0 40.0 30.0 22.0 15.0 9.0
Min. 100.0 90.0 77.0 53.0 33.0 21.0 14.0 9.0 6.0 4.0
Prosen lolos (%)

100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0
0.0 0.1 1.0 10.0 100.0

Grad. batas atas Ukuran Grad.


saringan
batas bawah (mm) Gradasi ranc angan

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis

Tanggal : Tanggal :

Tanda Tangan : Tanda Tangan :

Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng


No.Formulir : 03-5

FORMULIR Terbitan/Revisi : 1/0


: DSIP/F-IK-PJS-
Tanggal Revisi
03-5-25-16-01
PENGUJIAN BERAT JENIS Laboratorium Penguji
LAB.PENGUJIAN BALAI Halaman 1 dari 1
LITBANG PERKERASAN JALAN MAKSIMUM CAMPURAN BERASPAL LP-269-IDN

1. No. Order/Contoh : PKL SMKN 1 MAUMERE


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING
3. Jenis Pekerjaan 0
4. Diterima tanggal :
5. Di uji tanggal : 10 Maret 2017
6. Metode uji : SNI 03-6893-2002
7. Hasil pengujian :

Nomor contoh

No. Contoh
I II rata-rata

Berat fiqnometer + benda uji (gr) A 2410.5 2410.5

Berat fiqnometer (gr) B 1218.0 1218.0

Berat benda uji (gr) A-B=C 1178.3 1178.3

Berat fiqnometer + air (gr) D 3651.9 3651.9

Berat piqnometer + air + benda uji (gr) E 4350.2 4350.2

Volume benda uji (cc) (C + D) - E = F 480.0 480.0

GMM C/F 2.455 2.455 2.455

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis

Tanggal : Tanggal :

Tanda Tangan : Tanda Tangan :

Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng


Berat jenis Bulk Ag. Hotbin Gabungan

Proporsi Bj. Bulk Bj. Bulk Bj. Bulk agregat


No. Agregat
agregat agregat agregat Gabungan

1 Agregat KASAR 11.0% 2.641 4.17

2 Agregat SEDANG 34.0% 2.642 12.87

3 AGREGAT HALUS 55.0% 2.663 20.66

4 #REF! #REF! 2.640 #REF!

5 #REF! #REF! 3.15 #REF!

#REF! #REF! #REF!


No.Formulir : 03-5

FORMULIR Terbitan/Revisi : 1/0


Tanggal Revisi : DSIP/F-IK-PJS-03-5-25-10-01

LAB.PENGUJIAN BALAI PENGUJIAN MARSHALL Halaman 1 dari 2


LITBANG PERKERASAN JALAN

1. No. Order/Contoh : PKL SMKN 1 MAUMERE 5. Di uji tanggal : 10 Maret 2017


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING 6. Metode uji : AASHTO T 245-97 (2004)
3. Jenis Pekerjaan 0 7. Hasil pengujian :
4. Diterima tanggal :
Kal. Proving ring = 15.26

Kadar Aspal Berat Benda Uji Satabilitas


Berat Jenis Rongga Rongga Rongga
Hasil Kadar Tebal
Kode Isi Benda Campuran Dalam Terhadap Terisi
Kepadatan Kalibrasi Pelelehan Bagi Aspal Film
Briket thd Berat thd Berat Uji Maksimum Agregat Campuran Aspal Bacaan Setelah
Kering SSD Dalam Air Proving Marshall Effektif Aspal
Agregat Campuran (teoritis) (VMA) (VIM) (VFB) Pada Alat Dikoreksi
Ring

% % gr gr gr cc gr/cc % % % kg mm kg/mm % mikron


r=c-
c=100/ i=100/((100- j=100-(h* k=100- l=100* (j- n=m*kal o=n*kor.vo
a b d e f g=e-f h=d/g m p q=o/p ((x/100)* s
(100+b)*b c)/v+c/w) (100-c))/u) (100*(h/i) k)/j prov ring l
(100-c))
1 5.0 1171.0 1175.1 664.7 510.4 2.294 2.472 #REF! 7.19 #REF! 70 1068.2 1068.2 3.80 281.1 #REF! #REF!
2 5.0 1173.7 1177.2 666.3 510.9 2.297 2.472 #REF! 7.06 #REF! 74 1129.2 1129.2 3.50 322.6 #REF! #REF!
3 5.0 1172.6 1176.7 665.2 511.5 2.292 2.472 #REF! 7.26 #REF! 71 1083.5 1083.5 3.60 301.0 #REF! #REF!
5.0 2.295 2.472 #REF! 7.16 #REF! 1093.6 3.55 301.6 #REF! #REF!
1 5.5 1175.9 1178.3 669.6 508.7 2.312 2.455 #REF! 5.83 #REF! 76 1159.8 1159.8 3.50 331.4 #REF! #REF!
2 5.5 1172.1 1175.4 665.3 510.1 2.298 2.455 #REF! 6.40 #REF! 73 1114.0 1114.0 3.70 301.1 #REF! #REF!
3 5.5 1174.1 1178.1 668.1 510.0 2.302 2.455 #REF! 6.22 #REF! 71 1083.5 1083.5 3.90 277.8 #REF! #REF!
5.5 2.304 2.455 #REF! 6.31 #REF! 1136.9 3.80 289.4 #REF! #REF!
1 6.0 1172.8 1174.7 669.9 504.8 2.323 2.438 #REF! 4.70 #REF! 78 1190.3 1237.9 3.50 353.7 #REF! #REF!
2 6.0 1174.1 1176.3 670.2 506.1 2.320 2.438 #REF! 4.84 #REF! 76 1159.8 1206.2 3.60 335.0 #REF! #REF!
3 6.0 1173.3 1175.7 669.8 505.9 2.319 2.438 #REF! 4.87 #REF! 78 1190.3 1237.9 3.50 353.7 #REF! #REF!
6.0 2.320 2.438 #REF! 4.80 #REF! 1206.2 3.53 347.5 #REF! #REF!
1 6.5 1175.1 1177.2 670.1 507.1 2.317 2.421 #REF! 4.29 #REF! 67 1022.4 1063.3 3.90 272.6 #REF! #REF!
2 6.5 1170.9 1173.3 668.3 505.0 2.319 2.421 #REF! 4.24 #REF! 65 991.9 1031.6 4.00 257.9 #REF! #REF!
3 6.5 1172.4 1174.6 667.8 506.8 2.313 2.421 #REF! 4.45 #REF! 61 930.9 968.1 3.70 261.6 #REF! #REF!
6.5 2.318 2.421 #REF! 4.35 #REF! 1047.4 3.85 264.1 #REF! #REF!
1 7.0 1173.9 1175.5 668.1 507.4 2.314 2.405 #REF! 3.79 #REF! 59 900.3 936.4 4.10 228.4 #REF! #REF!
2 7.0 1171.8 1173.6 667.8 505.8 2.317 2.405 #REF! 3.66 #REF! 62 946.1 984.0 3.80 258.9 #REF! #REF!
3 7.0 1172.1 1173.8 668.0 505.8 2.317 2.405 #REF! 3.64 #REF! 60 915.6 952.2 3.90 244.2 #REF! #REF!
7.0 2.316 2.405 #REF! 3.70 #REF! 957.5 3.93 243.8 #REF! #REF!
Gmm * :2.455 Ka Gmm : 5.5 Bj. agregat bulk : #REF! Bj. agregat eff. : 2.658 Bj. aspal : 1.062 Abs. Aspal : #REF!
1. No. Order/Contoh : PKL SMKN 1 MAUMERE 5. Di uji tanggal : 10 Maret 2017
2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING 6. Metode uji : AASHTO T 245-97 (2004)
3. Jenis Pekerjaan 0 7. Hasil pengujian :
4. Diterima tanggal :
Kal. Proving ring = 15.26

Keterangan : f = isi (d-e) i = % rongga thd. agregat 100-(g*(100-b))/bj.bulk) o = kelelehan (mm)


a = % aspal terhadap agregat g = berat isi (c/f) j = % rongga thd. campuran 100-(100x(g/h) p = Hasil bagi Marshall
b = % aspal terhadap campuran h = berat jenis maksimum (teoritis) k = % rongga terisi aspal (100x(i-j))/i n / o (kg/mm)
c = berat kering (gr) l = pembacaan arloji stabilitas q = Kadar aspal eff. (%)
d = berat dalam keadaan jenuh (gr) 100 m = stabilitas (l x konversi) c-((Abs.aspal/100)*(100-c))
e = berat dalam air (gr) %agregat +
%aspal n = stabilitas (kg) r = Tebal film aspal (mikron)
BJ. agregat BJ. aspal m x koreksi benda uji 1000*(Pb-Pba)
SA*BJAspal*(100-Pb)

* Gmm : ditentukan dengan cara AASHTO T 209


pada kadar aspal optimum perkiraan (Pb) (100-Pb) *** Absorpsi aspal terhadap total agregat =
** BJ. Eff Agr =
Pb = 0,035(%CA)+0,045(%FA)+0,18(%FF)+K (100/Gmm)-(Pb/BJ.aspal) (BJ. Eff. agr - BJ. Bulk agr)
100 x x BJ. Aspal
K = 0,5-1 untuk Laston; 2-3 untuk Lataston (BJ. Eff. agr x BJ. Bulk agr)

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis

Tanggal : Tanggal :

Tanda Tangan : Tanda Tangan :

Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng


No.Formulir

FORMULIR Terbitan/Revisi

Tanggal Revisi

UJI CAMPURAN
LAB.PENGUJIAN BALAI Halaman 1 dari 1
LITBANG PERKERASAN JALAN DENGAN ALAT PRD

1. No. Order/Contoh : PKL SMKN 1 MAUMERE 5. Di uji tanggal : 10 Maret 2017


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING 6. Metode uji : SNI 06-2489-1991
3. Jenis Pekerjaan 0 7. Hasil pengujian :
4. Diterima tanggal :
Kal. Proving ring = 15.26
Kadar Aspal Berat Benda Uji
Berat Jenis Rongga Rongga Rongga
Kode Isi Benda Campuran Dalam Terhadap Terisi
Kepadatan
Briket thd Berat thd Berat Uji Maksimum Agregat Campuran Aspal
Kering SSD Dalam Air (teoritis) (VMA) (VIM) (VFB)
Agregat Campuran

% % gr gr gr cc gr/cc % % %

c=100/ i=100/((100- j=100-(h* k=100- l=100* (j-


a b d e f g=e-f h=d/g
(100+b)*b c)/v+c/w) (100-c))/u) (100*(h/i) k)/j

1 5.5 2661.5 2665.1 1524.1 1141.0 2.333 2.455 #REF! 4.98 #REF!

1 6.0 2656.5 2659.3 1530.5 1128.8 2.353 2.438 #REF! 3.47 #REF!

1 6.5 2652.9 2654.1 1531.2 1122.9 2.363 2.421 #REF! 2.42 #REF!

Gmm * :2.455 Ka Gmm : 5.5 Bj. agregat bulk : #REF! Bj. agregat eff. : 2.658 Bj. aspal : 1.062 Abs. Aspal : #REF!
Keterangan : f = isi (d-e) i = % rongga thd. agregat 100-(g*(100-b))/bj.bulk) o = kelelehan (mm)
a = % aspal terhadap agregat g = berat isi (c/f) j = % rongga thd. campuran 100-(100x(g/h) p = Hasil bagi Marshall
b = % aspal terhadap campuran h = berat jenis maksimum (teoritis) k = % rongga terisi aspal (100x(i-j))/i n / o (kg/mm)
c = berat kering (gr) l = pembacaan arloji stabilitas q = Kadar aspal eff. (%)
d = berat dalam keadaan jenuh (gr) 100 m = stabilitas (l x konversi) c-((Abs.aspal/100)*(100-c))
e = berat dalam air (gr) %agregat %aspal n = stabilitas (kg) r = Tebal film aspal (mikron)
+
BJ. agregat BJ. aspal m x koreksi benda uji 1000*(Pb-Pba)
SA*BJAspal*(100-Pb)

* Gmm : ditentukan dengan cara AASHTO T 209


pada kadar aspal optimum perkiraan (P b) (100-Pb) *** Absorpsi aspal terhadap total agregat =
** BJ. Eff Agr =
Pb = 0,035(%CA)+0,045(%FA)+0,18(%FF)+K (100/Gmm)-(Pb/BJ.aspal) (BJ. Eff. agr - BJ. Bulk agr)
100 x x BJ. Aspal
K = 0,5-1 untuk Laston; 2-3 untuk Lataston (BJ. Eff. agr x BJ. Bulk agr)

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis

Tanggal : Tanggal :

Tanda Tangan : Tanda Tangan :

Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng


No.Formulir
FORMULIR Terbitan/Revisi
Tanggal Revisi
GRAFIK
LAB.PENGUJIAN BALAI Halaman 1 dari 1
LITBANG PERKERASAN JALAN MARSHALL

1. No. Order/Contoh : PKL SMKN 1 MAUMERE 5. Di uji tanggal : 10 Maret 2017


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING 6. Metode uji : AASHTO T 245-97 (2004)
7. Hasil pengujian :
3. Jenis Pekerjaan 0
4. Diterima tanggal :
Kepadat an, gr/c c

f(x)24.00
=
2.340
22.00

VMA, %
20.00
2.320 18.00
f(x) = - 0.0112561857x^2 + 0.1462859849x + 1.843559521
16.00

2.300 14.00

12.00

2.280
10.00

4.5 5.0 5.5


Kadar aspal, %
6.0 6.5 7.0 7. 5 4.5 5.0 5.5 Kadar aspal,
6.0 % 6.5 7.0 7.5

f(x)
100 = 12

90 10
VFB, %

80 VIM, %
8
70
f(x)
6 = 0.4168637282x^2 - 6.7814137858x + 30.7353794952
60

50 f(x)
4 = 0.9365146479x^2 - 13.7935060582x + 52.5122735394

40 2

30 0
Kadar6.0
aspal, % Kadar aspal, %
4.5 5.0 5.5 6.5 7.0 7.5 4.5 5.0 5.5 6.0 6.5 7.0 7.5
Kelelehan, m m
Stabilitas, kg

1400 5
4.5
1300
4
1200 f(x)
3.5 = 0.0714285714x^2 - 0.6938095238x + 5.289047619
3
1100 f(x) = - 141.2349333333x^2 + 1622.4868x - 3491.52288 2.5
2
1000
1.5
900 1
0.5
800 0
Kadar aspal, %
4.5 5.0 5.5 6.0 6.5 7.0 7.5 4.5 5.0 5.5 Kadar aspal,
6.0 % 6.5 7.0 7.5
M a r s h a a l q u o t ie n t , k g / m m

K a d a r a s p a l e f e k t if

f(x) =
9.00

450 8.00

400 7.00

350 6.00

5.00
f(x) = 300
- 45.0442770886x^2 + 512.357917462x - 1140.7575943233
250 4.00
200 3.00
150 2.00
4.5 5. 0 5. 5 Kadar aspal,
6.0 % 6. 5 7. 0 7. 5 Kadar aspal, %
4.5 5.0 5.5 6.0 6.5 7. 0 7.5

10

Kepadatan 9
KAO 6.250 %
VMA 8 Kepadatan 2.326 t/m3
VIM Marshall 7 VMA 18.0 %
VIM PRD 6 VIMmarshall 4.6 %
VFB
5 VIMprd 2.9 %
Stabilitas
Stabilitas VFB 74.22 %
Kelelehan
4

Kelelehan Stabilitas 1381 kg


MQ
3

MQ
2
Kelelehan 3.73 mm
1
MQ 303 kg/mm
0
Stab. sisa 89.0 %
4.50 5.00 5.50 6.00 aspal, % 6.50
Kadar 7.00 7.50 k.asp efektif 6.13 mikron

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis

Tanggal : Tanggal :

Tanda Tangan : Tanda Tangan :

Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng


No.Formulir FT/5.4/1/Ag-01

FORMULIR Terbitan/Revisi 6/0


Tanggal Revisi 02/02/2009
UJI CAMPURAN
LAB.PENGUJIAN BALAI Halaman 1 dari 2
LITBANG PERKERASAN JALAN DENGAN ALAT MARSHALL

1. No. Order/Contoh : PKL SMKN 1 MAUMERE 5. Di uji tanggal : 25 Juli 2016


2. Jenis Contoh Uji : CAMPURAN BERASPAL AC WEARING 6. Metode uji : AASHTO T 245-97 (2004)
3. Jenis Pekerjaan 0 7. Hasil pengujian :
4. Diterima tanggal :
Kal. Proving ring = 15.26
Kadar Aspal Berat Benda Uji Satabilitas
Berat Jenis Rongga Rongga Rongga
Hasil Kadar Tebal
Kode Isi Benda Campuran Dalam Terhadap Terisi
Kepadatan Kalibrasi Pelelehan Bagi Aspal Film
Briket thd Berat thd Berat Uji Maksimum Agregat Campuran Aspal Bacaan Setelah
Kering SSD Dalam Air Proving Marshall Effektif Aspal
Agregat Campuran (teoritis) (VMA) (VIM) (VFB) Pada Alat Dikoreksi
Ring

% % gr gr gr cc gr/cc % % % kg mm kg/mm % mikron

r=c-
c=100/ i=100/((100- j=100-(h* k=100- l=100* (j-
a b d e f g=e-f h=d/g m n o=m*n p q=o/p ((x/100)* s
(100+b)*b c)/v+c/w) (100-c))/u) (100*(h/i) k)/j
(100-c))

Setelah direndam selama 1 x 30 menit pada suhu 60 oC


1 6.3 1173.2 1175.1 670.1 505.0 2.323 2.430 #REF! 4.38 #REF! 80 1220.8 1269.6 3.30 384.7 #REF! #REF!
2 6.3 1174.9 1176.8 670.7 506.1 2.321 2.430 #REF! 4.45 #REF! 79 1205.5 1253.8 3.60 348.3 #REF! #REF!
3 6.3 1177.5 1179.4 381.1 798.3 1.475 2.430 #REF! 39.29 #REF! 75 1144.5 1190.3 3.30 360.7 #REF! #REF!
6.3 2.322 2.430 #REF! 4.41 #REF! 1222.0 3.45 354.5 #REF! #REF!
Setelah direndam selama 1 x 24 Jam pada suhu 60 oC 89.0
1 6.3 1176.0 1178.1 680.9 497.2 2.365 2.43 #REF! 2.64 #REF! 67 1022.4 1063.3 3.70 287.4 #REF! #REF!
2 6.3 1178.9 1180.3 681.7 498.6 2.364 2.43 #REF! 2.68 #REF! 69 1052.9 1095.1 3.70 296.0 #REF! #REF!
3 6.3 1178.8 1180.6 681.9 498.7 2.364 2.43 #REF! 2.71 #REF! 68 1037.7 1079.2 4.00 269.8 #REF! #REF!
6.3 2.365 2.430 #REF! 2.66 #REF! 1087.1 3.85 282.9 #REF! #REF!
Gmm * :2.455 Ka Gmm : 5.5 Bj. agregat bulk : #REF! Bj. agregat eff. : 2.658 Bj. aspal : 1.062 Abs. Aspal : #REF!
Keterangan : f = isi (d-e) i = % rongga thd. agregat 100-(g*(100-b))/bj.bulk) o = kelelehan (mm)
a = % aspal terhadap agregat g = berat isi (c/f) j = % rongga thd. campuran 100-(100x(g/h) p = Hasil bagi Marshall
b = % aspal terhadap campuran h = berat jenis maksimum (teoritis) k = % rongga terisi aspal (100x(i-j))/i n / o (kg/mm)
c = berat kering (gr) l = pembacaan arloji stabilitas q = Kadar aspal eff. (%)
d = berat dalam keadaan jenuh (gr) 100 m = stabilitas (l x konversi) c-((Abs.aspal/100)*(100-c))
e = berat dalam air (gr) %agregat %aspal n = stabilitas (kg) r = Tebal film aspal (mikron)
+
BJ. agregat BJ. aspal m x koreksi benda uji 1000*(Pb-Pba)
SA*BJAspal*(100-Pb)
* Gmm : ditentukan dengan cara AASHTO T 209
pada kadar aspal optimum perkiraan (Pb) (100-Pb) *** Absorpsi aspal terhadap total agregat =
Pb = 0,035(%CA)+0,045(%FA)+0,18(%FF)+K ** BJ. Eff Agr = (100/Gmm)-(Pb/BJ.aspal) (BJ. Eff. agr - BJ. Bulk agr)
100 x x BJ. Aspal
K = 0,5-1 untuk Laston; 2-3 untuk Lataston (BJ. Eff. agr x BJ. Bulk agr)

Bandung, 23 Maret 2017

Diperiksa Oleh Penyelia Manager Teknis


Tanggal : Tanggal :
Tanda Tangan : Tanda Tangan :
Nama : Ilham Hermawan, S.ST Nama : Hendri Hadisi, S.Si., M.Eng
TIMBANGAN BAHAN AGREGAT MARSHALL
CAMPURAN BERASPAL AC - WC

5.0% 5.5% 6.0% 6.5% 7.0%


Kadar Aspal Rencana
marshall marshall marshall marshall marshall

Total campuran 1190 1190 1190 1190 1190


Aspal murni 59.5 65.5 71.4 77.4 83.3

Total aspal 59.5 65.5 71.4 77.4 83.3

Berat Agregat 1130.5 1124.6 1118.6 1112.7 1106.7

Agregat KASAR 11.0% 124.4 123.7 123.0 122.4 121.7


Agregat SEDANG 34.0% 384.4 382.3 380.3 378.3 376.3
AGREGAT HALUS 55.0% 621.8 618.5 615.2 612.0 608.7

Berat Komulatif Agregat


Agregat KASAR 124.4 123.7 123.0 122.4 121.7
Agregat SEDANG 508.7 506.0 503.4 500.7 498.0
AGREGAT HALUS 1130.5 1124.6 1118.6 1112.7 1106.7

TIMBANGAN BAHAN AGREGAT PRD


CAMPURAN BERASPAL AC - WC

5.0% 5.5% 6.0% 6.5% 7.0%


Kadar Aspal Rencana
marshall marshall marshall marshall marshall

Total campuran 2700 2700 2700 2700 2700


Aspal murni 135.0 148.5 162.0 175.5 189.0

Total aspal 135.0 148.5 162.0 175.5 189.0

Berat Agregat 2565.0 2551.5 2538.0 2524.5 2511.0

Agregat KASAR 11.0% 282.2 280.7 279.2 277.7 276.2


Agregat SEDANG 34.0% 872.1 867.5 862.9 858.3 853.7
AGREGAT HALUS 55.0% 1410.8 1403.3 1395.9 1388.5 1381.1

Berat Komulatif Agregat


Agregat KASAR 282.2 280.7 279.2 277.7 276.2
Agregat SEDANG 1154.3 1148.2 1142.1 1136.0 1130.0
AGREGAT HALUS 2565.0 2551.5 2538.0 2524.5 2511.0
2.325813
10675.48

Anda mungkin juga menyukai