Anda di halaman 1dari 4

EPC PEMBANGUNAN OPEN ACCESS

PT. PERTAMINA (PERSERO)


RU - VII KASIM

Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens


Designation: C 39/C 39M – 01
Kontraktor : PT. HK - PT.GSB, JO Petugas Tes : BINTANG
Pekerjaan : Uji coba Cetakan : Selinder - ASTM C 470
Mutu rencana : 15 Mpa Dimensi : 15 x 30
Elemen struktur : Lean concrete L/D : 1
MIX DESAIN ACI 211.1-91 Faktor : 0.87
DESAIN PROPORSI BAHAN CAMPURAN BETON 1-m3 HASIL UJI COBA
Ref.
MSA W/C S/A A/C Air Semen Silika Fume Pasir Batu Pecah Admixture Slump Temp.
No. mm % % % kg kg kg kg kg kg cm ⁰C
TM 01 20 60.00 41.71 2.00 185 308 722 1009 0.77 12 30.2
No. Urut 1 2 3 KALIBRASI POLA RETAK
Berat sampel ( gr ) 11750 11748 11672 Mesin Kapasitas 2000kN
A . Pembacaan beban ( kN ) 285 310 300 Seri n.2810074 - Analog A B C D E
B . Persen Kesalahan (%) 0.006
Nilai U₉₅% = ± 0.6% (k=2)
E . Beban terkoreksi A-B 284.99 309.99 299.99
Luas
Beban Kuat Persen
Ref. Identifikasi Pola Alas Kuat
Tanggal Umur Koef. Berat Isi Maksimum Tekan Ep terhadap
No. benda uji Retak Tekan fc' - fc'r (fc' - fc'r)²
(N) (N/mm2) Umur
(mm²)
n id buat tes r hari g g/cm3 A P P/A 100(A-B)/B Mpa %
1 22-Mar-22 25-Mar-22 B 3 0.46 2.216 17671.5 284994 16.13 0.0021 16.13 108 -0.75 0.57
2 22-Mar-22 25-Mar-22 B 3 0.46 2.216 17671.5 309994 17.54 0.0019 17.54 117 0.66 0.44
3 22-Mar-22 25-Mar-22 C 3 0.46 2.202 17671.5 299994 16.98 0.0020 16.98 113 0.09 0.01
Jumlah S 50.65 1.01
Standar Deviasi (S) Kuat Tekan Karakteristik (fc')
Kuat Tekan Rata - Rata ( fc'r ) 16.88 Mpa
Perkiraan kuat tekan di 28 hari 36.70 Mpa
 ( fc  fcr ) 2 fcr
S  = K  1,64.S = Catatan : Kecepatan pembebanan benda uji terhadap kuat tekan
n 1 n Benda Uji Silinder 0.25 ± 0.05 Mpa/detik - ASTM 39/C39M - 05

Witnessed and Approved by Witnessed and Checked by Created and Prepared by


Owner Contractor Concrete Supply
PT. Pertamina Persero Tbk. PT. HK - PT. GSB, KSO PT. Cipta Beton Sinar Perkasa
Date : Date : Date :
Sign : Sign : Sign :

Name Name Name


EPC PEMBANGUNAN OPEN ACCESS
PT. PERTAMINA (PERSERO)
RU - VII KASIM

Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens


Designation: C 39/C 39M – 01
Kontraktor : PT. HK - PT.GSB, JO Petugas Tes : BINTANG
Pekerjaan : Uji coba Cetakan : Selinder - ASTM C 470
Mutu rencana : 29 Mpa Dimensi : 15 x 30
Elemen struktur : Building, Foundation, Pit, Ditch L/D : 1
MIX DESAIN ACI 211.1-91 Faktor : 0.87
DESAIN PROPORSI BAHAN CAMPURAN BETON 1-m3 HASIL UJI COBA
Ref.
MSA W/C S/A A/C Air Semen Silika Fume Pasir Batu Pecah Admixture Slump Temp.
No. mm % % % kg kg kg kg kg kg cm ⁰C
TM 02 20 0.44 37.98 2.00 185 420 20 618 1009 1.26 12 28.8
No. Urut 1 2 3 KALIBRASI POLA RETAK
Berat sampel ( gr ) 11887 11795 11747 Mesin Kapasitas 2000kN
A . Pembacaan beban ( kN ) 395 620 540 Seri n.2810074 - Analog A B C D E
B . Persen Kesalahan (%) 0.006
Nilai U₉₅% = ± 0.6% (k=2)
E . Beban terkoreksi A-B 394.99 619.99 539.99
Luas
Beban Kuat Persen
Ref. Identifikasi Pola Alas Kuat
Tanggal Umur Koef. Berat Isi Maksimum Tekan Ep terhadap
No. benda uji Retak Tekan fc' - fc'r (fc' - fc'r)²
(N) (N/mm2) Umur
(mm²)
n id buat tes r hari g g/cm3 A P P/A 100(A-B)/B Mpa %
1 22-Mar-22 25-Mar-22 E 3 0.46 2.242 17671.5 394994 22.35 0.0015 22.35 77 -6.98 48.71
2 22-Mar-22 25-Mar-22 B 3 0.46 2.225 17671.5 619994 35.08 0.0010 35.09 121 5.75 33.10
3 22-Mar-22 25-Mar-22 B 3 0.46 2.216 17671.5 539994 30.56 0.0011 30.56 105 1.23 1.50
Jumlah S 88.00 83.30
Standar Deviasi (S) Kuat Tekan Karakteristik (fc')
Kuat Tekan Rata - Rata ( fc'r ) 29.33 Mpa
Perkiraan kuat tekan di 28 hari 63.77 Mpa
 ( fc  fcr ) 2 fcr
S  = K  1,64.S = Catatan : Kecepatan pembebanan benda uji terhadap kuat tekan
n 1 n Benda Uji Silinder 0.25 ± 0.05 Mpa/detik - ASTM 39/C39M - 05

Witnessed and Approved by Witnessed and Checked by Created and Prepared by


Owner Contractor Concrete Supply
PT. Pertamina Persero Tbk. PT. HK - PT. GSB, KSO PT. Cipta Beton Sinar Perkasa
Date : Date : Date :
Sign : Sign : Sign :

Name Name Name


EPC PEMBANGUNAN OPEN ACCESS
PT. PERTAMINA (PERSERO)
RU - VII KASIM

Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens


Designation: C 39/C 39M – 01
Kontraktor : PT. HK - PT.GSB, JO Petugas Tes : BINTANG
Pekerjaan : Uji coba Cetakan : Selinder - ASTM C 470
Mutu rencana : 29 Mpa Dimensi : 15 x 30
Elemen struktur : Building, Foundation, Pit, Ditch L/D : 1
MIX DESAIN ACI 211.1-91 Faktor : 0.87
DESAIN PROPORSI BAHAN CAMPURAN BETON 1-m3 HASIL UJI COBA
Ref.
MSA W/C S/A A/C Air Semen Silika Fume Pasir Batu Pecah Admixture Slump Temp.
No. mm % % % kg kg kg kg kg kg cm ⁰C
TM 03 20 60.00 37.68 2.00 185 430 20 610 1009 1.29 12 28.8
No. Urut 1 2 3 KALIBRASI POLA RETAK
Berat sampel ( gr ) 11813 11908 11849 Mesin Kapasitas 2000kN
A . Pembacaan beban ( kN ) 520 480 565 Seri n.2810074 - Analog A B C D E
B . Persen Kesalahan (%) 0.006
Nilai U₉₅% = ± 0.6% (k=2)
E . Beban terkoreksi A-B 519.99 479.99 564.99
Luas
Beban Kuat Persen
Ref. Identifikasi Pola Alas Kuat
Tanggal Umur Koef. Berat Isi Maksimum Tekan Ep terhadap
No. benda uji Retak Tekan fc' - fc'r (fc' - fc'r)²
(N) (N/mm²) Umur
(mm²)
n id buat tes r hari g g/cm3 A P P/A 100(A-B)/B Mpa %
1 22-Mar-22 25-Mar-22 B 3 0.46 2.228 17671.5 519994 29.43 0.0012 29.43 101 -0.09 0.01
2 22-Mar-22 25-Mar-22 C 3 0.46 2.246 17671.5 479994 27.16 0.0013 27.16 94 -2.36 5.56
3 22-Mar-22 25-Mar-22 C 3 0.46 2.235 17671.5 564994 31.97 0.0011 31.97 110 2.45 6.01
Jumlah S 88.56 11.58
Standar Deviasi (S) Kuat Tekan Karakteristik (fc')
Kuat Tekan Rata - Rata ( fc'r ) 29.5 Mpa
Perkiraan kuat tekan di 28 hari 64.2 Mpa
 ( fc  fcr ) 2 fcr
S  = K  1,64.S = Catatan : Kecepatan pembebanan benda uji terhadap kuat tekan
n 1 n Benda Uji Silinder 0.25 ± 0.05 Mpa/detik - ASTM 39/C39M - 05

Witnessed and Approved by Witnessed and Checked by Created and Prepared by


Owner Contractor Concrete Supply
PT. Pertamina Persero Tbk. PT. HK - PT. GSB, KSO PT. Cipta Beton Sinar Perkasa
Date : Date : Date :
Sign : Sign : Sign :

Name Name Name


EPC PEMBANGUNAN OPEN ACCESS
PT. PERTAMINA (PERSERO)
RU - VII KASIM

PHOTO DOKUMENTASI UJI TEKAN


Location : EPC RU-VII KASIM Lab CBSP Trial Date : 22-Mar-22
Sources : Tandeki - Manado and Bula - Seram Testing Date : 25-Mar-22
Material : Fine Aggregate and Coarse Aggregate Age : 3

Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens


Designation: C 39/C 39M – 01
Hasil Uji Kuat Tekan 15Mpa Cement 308kg/m3
Sampel Ref. No. 01 Sampel Ref. No. 02 Sampel Ref. No. 03

Hasil Uji Kuat Tekan 29Mpa Cement 420kg/m3


Sampel Ref. No. 01 Sampel Ref. No. 02 Sampel Ref. No. 03

Hasil Uji Kuat Tekan 29Mpa Cement 430kg/m3


Sampel Ref. No. 01 Sampel Ref. No. 02 Sampel Ref. No. 03

Witnessed and Approved by Witnessed and Checked by Created and Prepared by


Owner Contractor Concrete Supply
PT. Pertamina Persero Tbk. PT. HK - PT. GSB, KSO PT. Cipta Beton Sinar Perkasa
Date : Date : Date :
Sign : Sign : Sign :

Name Name Name

Anda mungkin juga menyukai