Anda di halaman 1dari 4

Project : Sorik Merapi Ghoetermal Project JMF No.

:
Contractor : PT. Gumbot Raya Madina Rev :
Item of Work : JMF Beton K-300 Date : 24 December 2017
Rev. Date :

PERENCANAAN CAMPURAN BETON


NO. DISKRIPSI TABEL/GRAFIK/PERHITUNGAN PERHITUNGAN
1 KUAT TEKAN YANG DISYARATKAN DITETAPKAN 24.90 Mpa PADA 28 HARI
BAGIAN CACAT 5%
2 DEVIASI STANDAR 3.200 N/mm2 ATAU TANPA DATA
3 KONVERSI KE KUBUS DITETAPKAN 0.80
24.90 x 0.83 = 20.70 Mpa
4 NILAI TAMBAH (MARGIN) DITETAPKAN ( k = 1.64 )
1.640 x 3.20 = 5.20 Mpa
5 KUAT RATA-RATA YANG DITARGETKAN 20.70 + 5.20 = 25.90 Mpa
6 JENIS SEMEN DITETAPKAN SEMEN PORTLAND TYPE I
7 JENIS AGGREGATE KASAR BATU PECAH
JENIS AGGREGATE HALUS BATU PECAH DAN ALAMI
8 FAKTOR AIR - SEMEN BEBAS 47.000
9 FAKTOR AIR SEMEN MAKSIMUM 47.000
10 SLUMP DITETAPKAN SLUMP 140 -120,0 mm
11 UKURAN AGGREGATE MAKSIMUM DITETAPKAN 30,0 mm
12 KADAR AIR BEBAS TABEL 181.00 kg/m3
13 JUMLAH SEMEN (12) : (9) ATAU (12) : (8) 181.00 : 47.00 = 385 kg/m3
14 JUMLAH SEMEN MAKSIMUM DITETAPKAN 385 kg/m3
15 JUMLAH SEMEN MINIMUM 375 kg/m3
16 ADITIF (lt) 0.50 kg/m3 ( If Any )
17 SUSUNAN BESAR BUTIR AGGREGATE HALUS
18 PERSENT AGGREGATE KASAR 20 - 30 mm 60.7%
19 PERSENT AGGREGATE PASIR ALAM 39.3%
20 BERAT JENIS RELATIF, AGGREGATE DIKETAHUI
(KERING PERMUKAAN)
21 BERAT JENIS BETON STRANDAR PROPORSI 2,381 kg/m3
22 BERAT AGGREGATE GABUNGAN (21) - (13+14+16) 1,815 kg/m3
23 BERAT AGGREGATE KASAR 20 - 30 mm STRANDAR PROPORSI 1,102 kg/m3
24 BERAT AGGREGATE PASIR ALAM STRANDAR PROPORSI 713 kg/m3

PROPORSI CAMPURAN DALAM 1 M3


AIR AGGREGATE KASAR AGGREGATE KASAR 10 -
URAIAN SEMEN AGGREGATE PASIR ALAM
(LITER/KG) 20 - 30 mm 20 mm
BERAT (KG) 385.106 181.000 1,102 713
BERAT JENIS 3.15 1.000 2.534 2.609
UNIT WEIGT (gr/cm3) 1.25 1.000
VOLUME GEMBUR (M3) 0.308 0.181
VOLUME PADAT (M3) 0.122 0.181 0.435 0.273

A. Composisi Campuran Beton dalam Satuan Berat C. Composisi Campuran beton dalam mixer menggunakan 1 zak cement

Mix Uraian Vol. ( m3 ) Air Liter/Kg * Cement 50 Kg


1 Tone Cement 0.32 * Pasir 93 Kg
3.2 Tone Pasir 1.23 470 * Split 2/3 143 Kg
4 Tone Agregate 1.58 * Air 24 Liter

B. Composisi Campuran Beton Dalam Bucket Perbandingan Campuran untuk 1 Zak Cement
( 1 : 1,5 : 2 )
Bucket Exca. Pc 200 ( m3 ) =
Mix Air Liter/Kg
0,8 m3
1.0 Tone Cement
1.5 Bucket Pasir 470
2.0 Bucket Angregate

CONTRACTOR OWNER

Tested By QC PT. Gumbot Raya Madina PT. Sorik Merapi Ghoetermal Project

Name : Name :
Date : Date :

JMF GRM/JMF To SMGP K-300


JMF GRM/JMF To SMGP K-300
Project : Sorik Merapi Ghoetermal Project JMF No. :
Contractor : PT. Gumbot Raya Madina Rev :
Item of Work : JMF Beton K-225 Date : 24 December 2017
Rev. Date :

PERENCANAAN CAMPURAN BETON


NO. DISKRIPSI TABEL/GRAFIK/PERHITUNGAN PERHITUNGAN
1 KUAT TEKAN YANG DISYARATKAN DITETAPKAN 225.00 Mpa PADA 28 HARI
BAGIAN CACAT 5%
2 DEVIASI STANDAR 2.300 N/mm2 ATAU TANPA DATA
3 KONVERSI KE KUBUS DITETAPKAN 0.80
225.00 x 0.83 = 186.80 Mpa
4 NILAI TAMBAH (MARGIN) DITETAPKAN ( k = 1.64 )
1.640 x 2.30 = 3.80 Mpa
5 KUAT RATA-RATA YANG DITARGETKAN 186.80 + 3.80 = 190.60 Mpa
6 JENIS SEMEN DITETAPKAN SEMEN PORTLAND TYPE I
7 JENIS AGGREGATE KASAR BATU PECAH
JENIS AGGREGATE HALUS BATU PECAH DAN ALAMI
8 FAKTOR AIR - SEMEN BEBAS 47.000
9 FAKTOR AIR SEMEN MAKSIMUM 47.000
10 SLUMP DITETAPKAN SLUMP 140 -120,0 mm
11 UKURAN AGGREGATE MAKSIMUM DITETAPKAN 30,0 mm
12 KADAR AIR BEBAS TABEL 181.00 kg/m3
13 JUMLAH SEMEN (12) : (9) ATAU (12) : (8) 181.00 : 47.00 = 385 kg/m3
14 JUMLAH SEMEN MAKSIMUM DITETAPKAN 385 kg/m3
15 JUMLAH SEMEN MINIMUM 375 kg/m3
16 ADITIF (lt) 0.50 kg/m3 ( If Any )
17 SUSUNAN BESAR BUTIR AGGREGATE HALUS
18 PERSENT AGGREGATE KASAR 20 - 30 mm 60.0%
19 PERSENT AGGREGATE PASIR ALAM 40.0%
20 BERAT JENIS RELATIF, AGGREGATE DIKETAHUI
(KERING PERMUKAAN)
21 BERAT JENIS BETON STRANDAR PROPORSI 2,381 kg/m3
22 BERAT AGGREGATE GABUNGAN (21) - (13+14+16) 1,829 kg/m3
23 BERAT AGGREGATE KASAR 20 - 30 mm STRANDAR PROPORSI 1,097 kg/m3
24 BERAT AGGREGATE PASIR ALAM STRANDAR PROPORSI 732 kg/m3

PROPORSI CAMPURAN DALAM 1 M3


AIR AGGREGATE KASAR AGGREGATE KASAR 10 -
URAIAN SEMEN AGGREGATE PASIR ALAM
(LITER/KG) 20 - 30 mm 20 mm
BERAT (KG) 371.000 181.000 1,097 732
BERAT JENIS 3.15 1.000 2.534 2.609
UNIT WEIGT (gr/cm3) 1.25 1.000
VOLUME GEMBUR (M3) 0.297 0.181
VOLUME PADAT (M3) 0.118 0.181 0.433 0.281

A. Composisi Campuran Beton dalam Satuan Berat C. Composisi Campuran beton dalam mixer menggunakan 1 zak cement

Mix Uraian Vol. ( m3 ) Air Liter/Kg * Cement 50 Kg


1 Tone Cement 0.32 * Pasir 114 Kg
3.2 Tone Pasir 1.99 470 * Split 2/3 171 Kg
4 Tone Agregate 2.76 * Air 28 Liter

B. Composisi Campuran Beton Dalam Bucket Perbandingan Campuran untuk 1 Zak Cement
( 1 : 2.5 : 3.5 )
Bucket Exca. Pc 200 ( m3 ) =
Mix Air Liter/Kg
0,8 m3
1.0 Tone Cement
2.5 Bucket Pasir 470
3.5 Bucket Angregate

CONTRACTOR OWNER

Tested By QC PT. Gumbot Raya Madina PT. Sorik Merapi Ghoetermal Project

Name : Name :
Date : Date :

JMF GRM/JMF To SMGP K-225