Anda di halaman 1dari 45

DUTCH CONE PENETROMETER

PROJECT PRAKTIKUM LABORATORIUM MEKANIKA TANAH


LOCATION LABORATORIUM MEKANIKA TANAH
DATE
TESTING METHOD SONDIR
DIAMETER KONUS (DC)=DS 3.57 Cm
PANJANG SELIMUT GESER (Ls) 13.35 Cm
DIAMETER PISTON (Dpi) 5.05 cm
LUAS PENAMPANG PISTON (Api) 20 Cm2
LUAS PENAMPANG KONUS (Ac) 10 Cm2
LUAS SELIMUT GESER (As) 149.65 cm2
Kw qc fs Lf Rf
Depth Cw Tw (Tw-Cw) (Cw.Api)/Ac Kw.Api/As fs*20 Tf (fs/qc)*100
No.
(m) (kg/cm2) (kg/cm2) (kg/cm2) (kg/cm2) (kg/cm2) (kg/cm) (kg/cm) (%)
1 2 3 4 5 6 7 8 9
1 0 0 0 0 0 0.00 0.00 0 0.00
2 0.2 5 8 3 10 0.40 8.03 8.03 4.01
3 0.4 10 16 6 20 0.80 16.05 24.08 4.01
4 0.6 16 22 6 32 0.80 16.05 40.13 2.51
5 0.8 18 25 7 36 0.94 18.73 58.86 2.60
6 1 25 31 6 50 0.80 16.05 74.91 1.60
7 1.2 32 38 6 64 0.80 16.05 90.97 1.25
8 1.4 40 47 7 80 0.94 18.73 109.70 1.17
9 1.6 46 52 6 92 0.80 16.05 125.75 0.87
10 1.8 50 56 6 100 0.80 16.05 141.80 0.80
11 2 57 63 6 114 0.80 16.05 157.85 0.70
12 2.2 60 67 7 120 0.94 18.73 176.58 0.78
13 2.4 65 73 8 130 1.07 21.40 197.99 0.82
14 2.6 70 79 9 140 1.20 24.08 222.07 0.86
15 2.8 85 92 7 170 0.94 18.73 240.79 0.55
16 3 95 102 7 190 0.94 18.73 259.52 0.49
17 3.2 105 112 7 210 0.94 18.73 278.25 0.45
18 3.4 115 123 8 230 1.07 21.40 299.65 0.47
19 3.6 125 132 7 250 0.94 18.73 318.38 0.37
20 3.8 135 141 6 270 0.80 16.05 334.44 0.30
21 4 145 155 10 290 1.34 26.75 361.19 0.46
22 4.2 160 168 8 320 1.07 21.40 382.60 0.33
23 4.4 175 180 5 350 0.67 13.38 395.97 0.19
24 4.6 180 190 10 360 1.34 26.75 422.73 0.37
25 4.8 192 200 8 384 1.07 21.40 444.13 0.28

444.13 4.01

Tabel 1. Penafsiran Hasil Penyelidikan Tanah dengan Memakai Alat Sondir


Hasil Sondir (kg/cm2)
Klasifikasi
qc Fs
6 0,15 - 0,40 Humus, lempung sangat lunak
0.2 Pasir kelanauan lepas, pasir sangat lepas
6 - 10'
0,20 - 0,60 Lempung lembek, lempung kelanauan lembek
0.10 kerikil lepas
0,10 - 0,40 Pasir lepas
10 - 30'
0,40 - 0,80 Lempung atau lempung kelanauan
0,80 - 2,00 Lempung agak kenyal
1.50 Pasir kelanauan, pasir agak padat
30 - 60
1,50 - 3,00 Lempung atau lempung kelanauan kenyal
1.00 Kerikil kepasiran lepas
pasir padat, pasir kelanauan atau lempung padat dan
60 - 150 1,00 - 3,00
kerikil kelempungan
3.00 Lempung kerikil kenyal
150 - 300 1,00 - 2,00 Pasir padat, pasir kerikil padat , pasir kasar padat, pasir
kelanauan sangat padat
Ket :
qc= Tekanan Konus
fs= Hambatan Pelekat
(Sumber : Ir. Sunggono kh (1995), Buku Teknik Sipil, Penerbit NOVA, Bandung )
Hubungan Antara Rf dengan kedalaman hubugan antara perlawanankonus
angka banding geser (rf) kedalaman(m)
0 100
gesekan
200
total
300
(tf))
0
0.00 0.50 1.00 1.50 2.00 2.50 3.00 3.50 4.00 4.50 5.00
0 0.2
0.2 0.4

0.4 0.6
0.8
0.6
1
0.8
1.2
1
1.4
1.2
1.6
1.4
1.8
1.6 2
1.8 2.2

kedalaman
2 2.4
2.2 2.6
Kedalaman

2.4 2.8
2.6 3

2.8 3.2

3 3.4
3.6
3.2
3.8
3.4
4
3.6
4.2
3.8
4.4
4
4.6
4.2 4.8
4.4 5
4.4
4
4.6
4.2 4.8
4.4 5
4.6
4.8
5
hubugan antara total hambatan pelekat degan
anankonus(qc) degan kedalaman(m)
an(m)
otal
300
(tf)) 400 500 600 0
0 50 100 150 200 250 300 350 400 450

0.2
0.4
0.6
0.8
1
1.2
1.4
1.6
1.8
2
2.2
kedalaman

2.4
2.6
2.8
3
3.2
3.4
3.6
3.8
4
4.2
4.4
4.6
4.8
5
4.4
4.6
4.8
5

perlawanan konus (qc)


GRAFIK HUBUNGAN KEDALAMAN DENGAN GESERAN TOTAL
Hasil Sondir (kg/cm2)
Klasifikasi
qc Fs
6 0,15 - 0,40 Humus, lempung sangat lunak
0.2 Pasir kelanauan lepas, pasir sangat lepas
6 - 10'
0,20 - 0,60 Lempung lembek, lempung kelanauan lembek
0.10 kerikil lepas
0,10 - 0,40 Pasir lepas
10 - 30'
0,40 - 0,80 Lempung atau lempung kelanauan
0,80 - 2,00 Lempung agak kenyal
1.50 Pasir kelanauan, pasir agak padat
30 - 60
1,50 - 3,00 Lempung atau lempung kelanauan kenyal
1.00 Kerikil kepasiran lepas
pasir padat, pasir kelanauan atau lempung padat dan
60 - 150 1,00 - 3,00
kerikil kelempungan
3.00 Lempung kerikil kenyal
150 - 300 1,00 - 2,00 Pasir padat, pasir kerikil padat , pasir kasar padat, pasir
kelanauan sangat padat
Tabel Pemeriksaan Berat Jenis

No. Percobaan Satuan I II


Berat Piknometer, W1 (gram) gram 29.1 39.3
Berat Piknometer + air, W2 (gram) gram 69 130
Berat Piknometer + air, + tanah W3 (gram) gram 98 158
Berat tanah kering, Ws (gram) gram 50 50
Temperatur, ℃ ℃ 26 26
Faktor koreksi, a = yT/y20 - 0.99682 0.99682
Berat Jenis, Gs - 2.38 2.27
Berat Jenis Rata-rata - 2.33
Tabel Pemeriksaan Kadar Air dan Berat Isi

Sampel - I II
Ring/Container Number - 1 2
Weight Ring (1) gram 29 39.6
Weight of Container (2) gram 84 64.2
Weight Ring + Container + Wet Soil (3) gram 208 187
Weight of Wet Soil (4) = (3)-(2)-(1) gram 95 83.2
Volume of Soil (5) cm3 58.20 57.3
Weight of Ring + Container + DrySoil (6) gram 192 159.5
Weight of Dry Soil (7) = (6)-(1)-(2) gram 79 55.7
Weight of Water (8) = (4)-(7) gram 16 27.5
Spesific Gravity, Gs - 2.33 2.68
Volume of Dry Soil (9) = (7)/Gs cm3 34.0 20.8
Volume of Pore (10) = (5)-(9) cm3 24.2 36.5
Wet Density, ywet = (4)/(5) gr/cm3 1.63 1.5
Water Content, w = (8)/(7)*100% % 20.3 49.4
Dry Density, gdry =ywet/(1+w) gr/cm3 1.36 0.97
Porosity, n = (10)/(5)*100% % 41.66 63.73
Degree of Saturation, Sr = (8)/(10)*100% % 65.98 75.31
*
Tabel Pemeriksaan Batas Cair

No Test Satuan 1 2 3
Jumlah Pukulan - 45 30 24
No. Container - I II III
Berat Tanah Basah + Container, W1 gram 42.4 53 52

Berat Tanah Kering + Container, W2 gram 35 43 42


Berat Container, W3 gram 11 13 18
Berat Air (Ww=W1-W2) gram 7.4 10 10
Berat Tanah Kering, (Wd=W2-W3) gram 24 30 24
Kadar Air, Ww/Wd x 100% % 30.83 33.33 41.67
Kadar air rata-rata % 40.74

GRAFIK BATAS CAIR


60.00
f(x) = − 18.3614597016996 ln(x) + 98.9888874428763
50.00

40.00
KADAR AIR

30.00

20.00

10.00

0.00
1 10 100
JUMLAH PUKULAN

Persamaan Regresi Grafik Batas Cair


Y = -18,36LN(X)+98,989 = 39.89

No x y ln(x) ln(x)^2
1 45 30.83 3.81 14.49
2 30 33.33 3.40 11.57
3 24 41.67 3.18 10.10
4 10 57.14 2.30 5.30
Jumlah 109 162.98 12.69 41.46
161.00
b = n. (Σln(x).y)-(Σln(x)).Σy)
n. (Σ(ln(x))^2)-(Σln(x))^2

= 4.(494,74)-(12,69)(162,98)
4.(41,46)-(161,00)

= -88.96
= -18.36
4.84

a = y'-bx
y' = Σy 162.98
=
n 4

x' = Σln(x) 12.69


=
n 4

a = y'-bx
= 28,57-(--20,85 . 3,17)
= 98.99

y = b.ln(x)+a
= 39.89
Tabel Pemeriksaan Batas Plastis

4 No Test Satuan 1 2
10 109 No. Container - I II
IV Berat Tanah Basah + Container, W1 gram 37 37
46 Berat Tanah Kering + Container, W2 gram 33 33

34 Berat Container, W3 gram 15.2 15.3


13 Berat Air (Ww=W1-W2) gram 4 4
12 Berat Tanah Kering, (Wd=W2-W3) gram 17.8 17.7
21 Kadar Air , Ww/Wd x 100% % 22.47 22.60
57.14 162.98 Kadar Air Rata-rata % 22.54
4 Index Plastisitas (PI=LL-PL) 18.21

98.9888874428763

100

ln(x)*y
117.37
113.37
132.42
131.58
494.74
= 40.74

= 3.17
Tabel Pemeriksaan Batas Susut

No Test Satuan 1 2
Berat Mould, W1 gram 3.1 3.9
Berat Mould + Tanah Basah, W2 gram 25.9 20.6
Berat Mould + Tanah Kering, W3 gram 14.9 13.1

Berat Air Raksa yang dipakai untuk mengisi


gram 335.2 334.1
mangkok shringkage, W4
Berat Air Raksa yang dipindahkan oleh tanah yang
gram 115.1 92.6
ditest, W5
Berat tanah basah, Ww=W2-W1 gram 22.8 16.7
Berat tanah kering, Wd=W3-W1 gram 11.8 9.2
Berat Air, Wa=W2-W3 gram 11 7.5
Berat Cawan petri, Wp gram 20 20
Berat jenis air raksa, r 13.6 13.6
Volume tanah basah, Vw=(W4-Wp)/r Cm3 23.18 23.10
Volume tanah kering, Vd=(W5-Wp)/r Cm3 6.99 5.34
Kadar air, = Wa/Wd x 100% % 93.22 81.52
Batas susut,
% 91.85 79.59
SL= Kadar air - ((Vw-Vd)/Wd)x100%)
SL rata-rata % 85.72
Tabel Pemeriksaan Analisa Saringan

Berat Berat Saringan + Diameter Berat Tertahan


No.
Saringan Berat Tertahan (mm) (gram)
4 442 442 4.75 0
10 427 542 2 115
16 389 477 0.84 88
40 332 496 0.43 164
60 394 442 0.25 48
100 333 339 0.15 6
200 389 456 0.08 67
Pan 288 300 - 12
A B C
500
ANALISA SARINGAN
lisa Saringan
100 100
90
77
80

Berat Kumulatif Persen (%) 70

Persen Lolos (%)


59.4
(gram) Tertahan Lolos 60
0 0 100 50
115 23 77 40
26.6
203 40.6 59.4 30
367 73.4 26.6 17 15.8
20
415 83 17 10 2.4000000
421 84.2 15.8
0
488 97.6 2.4 10 1 0.1
500 100 0 Diameter Saringan (mm)
D E F
SA SARINGAN

D10

26.6

17 15.8

2.40000000000001

0.1 0.01
meter Saringan (mm)
Tabel Pengujian Sand Cone Test
Kelompok 2

Perhitungan Kepadatan Tanah


Berat Botol + Corong W1
Berat Botol + Corong + Air W2 (gr)
Berat Botol + Pasir Penuh + Corong W3 (gr)
Berat Pasir Dalam Corong W4 (gr)
Berat Tanah Basah + Kaleng Lapangan W5 (gr)
Berat Kosong Kaleng Lapangan W6 (gr)
Berat Botol + Corong + Pasir secukupnya +-3/4 W7 (gr)
Berat Sisa Pasir + Botol + Corong Dilapangan W8(gr)
Berat Sisa Pasir Di Lubang W9 (gr)
Berat Tanah Basah (Wwet) (gr)
Volume Sisa Pasir Di Lubang (V) (Cm3)

Kadar Air (w) (%)


Berat Isi Tanah Kering Pengujian Lapangan (Ydry fiel)(gram/cm3)

Berat Isi Tanah Kering Pengujian Laboratorium (Kompaksi)


(Ydry fiel)(gram/cm3)

Derajat kepadatan = Ydry fiel (lapangan)/Ydry fiel (kompaksi)*100%


nd Cone Test
k2

Satuan I
Gram 683.2

Gram 7489

gram 8064 Ysand = W3-W1

gram 1381 W2-W1

gram 3600 = 7493-682,9

gram 339.1 7489-682,9

gram 5278 Ysand = 1.08

gram 3750

gram 147

gram 3260.9

Cm3 135.5

% 41

gram/cm3 1.7

gram/cm3 1.54

% 106.9
Ywet = Wwet/V

= 24.1

B.TK.+B.T.BOX = 65 GRAM

B.TB + B.T.Box = 87 gram

B.T.Box = 11.8 gram

B.Tk = 53.2 gram B.Tk = (B.Tk. +B.T.Box) - B.Tbox

B.TB = 75.2 gram = 65-11,8 gram

= 75.2 gram = 53.2 gram

B.TB + B.T.Box = 87 gram

B.Tk + B.T.Box = 65 gram

Berat Air = 22 gram

Kadar Air = Berat Air x 100 %

B.Tk

= 41 %
Tabel Pengujian Kompaksi
Kelompok 2

Berat tanah gram 2000 2000 2000


Kadar air mula-mula % 0 0 0
Penambahan Air ml 300 360 420
Kadar air Akhir % 15 18 21

Berat Isi Basah (Wet Density)

No. Mould - 1 2 3
Berat Mould gram 1758 1758 1758
Berat Tanah basah + Mould gram 3117 3245 3246
Berat tanah basah, Wwet gram 1359 1487 1488
Volume Mould cm3 928 928 928
Berat Volume Basah
gr/cm3 1.46 1.60 1.60
ywet = Wwet/Vmould
Kadar Air (Wate
Kel

2000 2000 No. Container - 1A


0 0 Berat tanah basah + Container gram 35
480 540 Berat tanah kering + Container gram 30
24 27 Berat air gram 5
Berat Container gram 11
Berat tanah kering gram 19
Kadar air % 26.32
Kadar air rata-rata % 28.16
4 5
1758 1758
3365.0 3498 Berat Isi Kering
1607 1740 Berat Tanah Basah, Wwet
928 928 Kadar Air Rata-rata
Berat Kering Wdry=𝑊𝑤𝑒𝑡/(1+(𝑊/100))
1.73 1.88
Volume Mould
Berat Isi Kering Ydry
=𝑊𝑑𝑟𝑦/𝑉𝑚𝑜𝑢𝑙
Yw=Gs/(1+W).Gs 𝑑
Berat Jenis (Gs)

Berat Jenis (Gs) = 2.33


Kadar Air Optimum (Wopt) = 27.12
1.74

GRAFIK KOMPAKSI
2.0

1.8

f(x) = 0.00127349774517678 x² − 0.0705123608773935


1.6

1.4
r/cm3)

1.2
2.0

1.8

f(x) = 0.00127349774517678 x² − 0.0705123608773935


1.6

1.4

Kepadatan Kering (gr/cm3)


1.2

1.0

0.8
f(x) = − 0.00545706146425209 x + 0.932882736860585
0.6

0.4

0.2

0.0
20 25 30 35 40

Kadar Air (w) (%)


Kadar Air (Water Content)
Kelompok 2

1B 2A 2B 3A 3B 4A 4B 5A 5B
37 35 41 35.0 39 46 42 38 37
31 29 33 28 32 36 33 30 29
6 6 8 7 7 10 9 8 8
11 11 11 11 11 11 11 11 11
20 18 22 17 21 25 22 19 18
30.00 33.33 36.36 41.18 33.33 40.00 40.91 42.11 44.44
28.16 34.85 37.25 40.45 43.27

gram 1359 1487 1488 1607


% 28.16 34.85 37.25 40.45
gram 1294.29 1402.83 1390.65 1460.91
cm3 928 928 928 928
gr/cm3 1.39 1.51 1.50 1.57
gr/cm3 0.78 0.74 0.73 0.71
2.33 2.33 2.33 2.33

n x y
1 28.16 1.39
2 34.85 1.51
3 37.25 1.50
4 40.45 1.57
5 43.27 1.74
D= 100.9 mm Σn 5 183.99 7.72
t= 116.1 mm
r= 50.45
V= 927864 mm3 x
= 928 cm3 5 183.99 6904.49
183.99 6904.49 263601.25
6904.49 6904.49 10215205.94

5.62 5.62
RAFIK KOMPAKSI

Persamaan garis regresi (dari grafik)


y= 0.0013 x2 - 0.07050
49774517678 x² − 0.0705123608773935 x + 2.37943656615993 y' = 0.0026 x - 0.0705
49774517678 x² − 0.0705123608773935 x + 2.37943656615993
0= 0.0026 x - 0.0705
x= 27.12 %
Jadi, kadar air optimum dicapai pada 27,12% dan%berat
saat 25,96 dan isi kering
berat 0,00263,11
isi kering gr/

5706146425209 x + 0.932882736860585

35 40 45 50 55

Kadar Air (w) (%)


1740
43.27
1611.11
928
1.74
0.70
2.33

x2 y2 x3 x.y x4 x2.y
792.87 1.95 22325.47 39.28 628638.14 1105.98
1214.42 2.29 42320.59 52.69 1474808.40 1836.07
1387.93 2.25 51707.11 55.84 1926343.36 2080.18
1636.57 2.48 66206.71 63.70 2678362.18 2576.76
1872.71 3.01 81041.38 75.14 3507053.87 3251.72
6904.49 11.97 263601.25 286.64 10215205.94 10850.70

y
7.72
286.64
10850.70

7.72
286.64
10850.70

x + 2.3794
y= 1.42 gr/cm3
dan berat isi kering 0,0026 gr/cm³
( 10 x Tumbukan)
Densitas
Berat tanah basah + mold gram 7674
Berat mold gram 4157.6
Berat tanah basah gram 3516.4
Isi cetakan (V) cm 3
2186.54
Berat volume basah (𝛾wet) gram/cm3 1.61
Berat volume kering (𝛾dry) gram/cm3 1.28

Kadar air
No. cawan - 1A 1B
Berat tanah basah + cawan gram 59.30 60.50
Berat tanah kering + cawan gram 49.60 50.60
Berat air gram 9.70 9.90
Berat cawan gram 12.50 12.20
Berat tanah kering gram 37.10 38.40
Kadar air (w) % 26.15 25.78
Kadar air rata-rata % 25.96

Penetrasi, kalibrasi proving ring, lbs/Dev = 32.1314

penetrasi Pembacaan arloji ukur Beban penetrasi


Waktu beban
(menit)
mm devisi lb
0 0 0 0.00
1/4 0.330 1.9 61.05
1/2 0.635 4.0 128.53
1 1.27 8.0 257.05
1 1/2 1.905 10.0 321.31
2 2.54 10.4 334.17
3 3.81 10.6 340.59
4 5.08 10.8 345.41
6 7.62 20.9 671.55
8 10.16 20.3 652.27
10 12.7 20.5 658.69

10 Tumbukan
750.00
650.00
f(x) = − 4.41616173021715 x² + 103.654486649701 x + 59.4426305912575
550.00
)
10 Tumbukan
750.00
650.00
f(x) = − 4.41616173021715 x² + 103.654486649701 x + 59.4426305912575
550.00
Beban (lbs)

450.00
350.00
250.00
150.00
50.00
0 2 4 6 8 10 12 14
Penurunan (mm)

No. x y ln(x) (ln(x))^2 ln(x).y


1 0.33 61.0 -1.11 1.23 -67.68
2 0.64 128.5 -0.45 0.21 -58.37
3 1.27 257.1 0.24 0.06 61.44
4 1.91 321.3 0.64 0.42 207.08
5 2.54 334.2 0.93 0.87 311.50
6 3.81 340.6 1.34 1.79 455.59
7 5.08 345.4 1.63 2.64 561.40
8 7.62 671.5 2.03 4.12 1363.76
9 10.16 652.3 2.32 5.38 1512.25
10 12.70 658.7 2.54 6.46 1674.14
46.05 3770.6 10.11 23.17 6021.11

Penurunan (x)
Beban (lbs) CBR (%)
(mm)
2.54 95.42 3.18
5.08 89.29 1.98
Nilai CBR rata-rata: 2.58

n (ΣLn(x)y) - (ΣLn(x).Σy)
b=
n (Σ (Ln(x))² - (Σ Ln (x))²
10 6021.11 - 10.11 3770.62
b=
10 23.17 - 102.14
22102.78
b=
129.52
b= 170.65
a = y' - bx'
y' = Σy a= 377.06 - 170.65
n a= 377.06 - 172.47
y' = 3770.62 a= 204.59
10
y' = 377.06
y= -4,4162x2 + 103,65x + 59,443
x' = Σ ln(x) y= -8.832 x +
n = 95.42
x' = 10.11 = 89.29
10
x' = 1.01
( 25 x Tumbukan)
Densitas
Berat tanah basah + mold gram
Berat mold gram
Berat tanah basah gram
Isi cetakan (V) cm3
Berat volume basah (𝛾wet) gram/cm3
Berat volume kering (𝛾dry) gram/cm3

Kadar air
No. cawan -
Berat tanah basah + cawan gram
Berat tanah kering + cawan gram
Berat air gram
Berat cawan gram
Berat tanah kering gram
Kadar air (w) %
Kadar air rata-rata %

Penetrasi, kalibrasi proving ring, lbs/Dev =

penetrasi Pembacaan arloji ukur


Waktu beban
(menit)
in devisi
0 0 0
1/4 0.330 0.5
1/2 0.635 0.8
1 1.27 1.0
1 1/2 1.905 1.3
2 2.54 1.9
3 3.81 2.7
4 5.08 3.8
6 7.62 5.1
8 10.16 6.3
10 12.7 7.2

25 Tumbukan
290.00
250.00
210.00 f(x) = − 0.55784864950763 x² + 25.1858859475061 x + 2.96948791037727
)
25 Tumbukan
290.00
250.00
210.00 f(x) = − 0.55784864950763 x² + 25.1858859475061 x + 2.96948791037727

Beban (lbs)
170.00
130.00
90.00
50.00
10.00
0 2 4 6 8 10 12 14
Penurunan (mm)

No. x y ln(x)
1 0.33 16.1 -1.11
2 0.64 25.7 -0.45
3 1.27 32.1 0.24
4 1.91 41.8 0.64
5 2.54 61.0 0.93
6 3.81 86.8 1.34
7 5.08 122.1 1.63
8 7.62 163.9 2.03
9 10.16 202.4 2.32
10 12.70 231.3 2.54
46.05 983.2 10.11

Penurunan (x) Beban


(mm) (lbs) CBR (%)

2.54 24.15 0.80


5.08 23.37 0.52
Nilai CBR rata-rata: 0.66

n (ΣLn(x)y) - (ΣLn(x).Σy)
b=
n (Σ (Ln(x))² - (Σ Ln (x))²
10 1766.61 -
b=
10 23.17 -
7729.06
b=
129.52
b= 59.67
a = y' - bx'
1.01 y' = Σy a= 98.32
n a= 98.32
y' = 983.22 a= 38.01
10
y' = 98.32
y= -0,5578x2 + 25,186x + 2,96
103.65 x' = Σ ln(x) = -1.116
n = 24.15
x' = 10.11 = 23.37
10
x' = 1.01
5 x Tumbukan)
Densitas
8027 Berat tanah basah + mold
4329 Berat mold
3698 Berat tanah basah
2186.54 Isi cetakan (V)
1.69 Berat volume basah (𝛾wet)
1.25 Berat volume kering (𝛾dry)

Kadar air
2A 2B No. cawan
51.80 58.60 Berat tanah basah + cawan
42.30 46.60 Berat tanah kering + cawan
9.50 12.00 Berat air
15.70 13.00 Berat cawan
26.60 33.60 Berat tanah kering
35.71 35.71 Kadar air (w)
35.71 Kadar air rata-rata

32.1314 Penetrasi, kalibrasi proving ring, lbs/Dev =

Beban penetrasi Waktu


(menit)
lb
0.00 0
16.07 1/4
25.71 1/2
32.13 1
41.77 1 1/2
61.05 2
86.75 3
122.10 4
163.87 6
202.43 8
231.35 10

60 Tum
1230.00
59475061 x + 2.96948791037727 f(x) = − 10.9986612024668 x
1030.00
60 Tum
1230.00
59475061 x + 2.96948791037727 f(x) = − 10.9986612024668 x
1030.00
830.00

Beban (lbs)
630.00
430.00
230.00

10 12 14 30.00
0 2 4
Penu

(ln(x))^2 ln(x).y No.


1.23 -17.81 1
0.21 -11.67 2
0.06 7.68 3
0.42 26.92 4
0.87 56.91 5
1.79 116.05 6
2.64 198.45 7
4.12 332.78 8
5.38 469.32 9
6.46 587.99 10
23.17 1766.61

Penurunan (x)
(mm)
2.54
5.08
Nilai CBR rata-rata:

b=

10.11 983.22
b=
102.14
b=

b=

- 59.67 1.01 y' =


- 60.31
y' =

y' =
-0,5578x2 + 25,186x + 2,9695
x + 25.186 x' =

x' =

x' =
( 60 x Tumbukan)

ah basah + mold gram 6683


ld gram 4343
ah basah gram 2340
an (V) cm 3
2186.54
ume basah (𝛾wet) gram/cm3 1.07
ume kering (𝛾dry) gram/cm3 0.79

n - 3A 3B
ah basah + cawan gram 70.00 73.40
ah kering + cawan gram 54.70 57.30
gram 15.30 16.10
wan gram 12.40 12.90
ah kering gram 42.30 44.40
r (w) % 36.17 36.26
r rata-rata % 36.22

i, kalibrasi proving ring, lbs/Dev = 32.1314

penetrasi Pembacaan arloji ukur Beban penetrasi


beban

in devisi lb
0 0 0.00
0.330 1.2 38.56
0.635 3 96.39
1.27 8.1 260.26
1.905 13.2 424.13
2.54 18.9 607.28
3.81 24 771.15
5.08 28.1 902.89
7.62 32 1028.20
10.16 35 1124.60
12.7 37.2 1195.29

60 Tumbukan
1230.00
f(x) = − 10.9986612024668 x² + 228.795146669203 x + 3.49481200157248
1030.00
60 Tumbukan
1230.00
f(x) = − 10.9986612024668 x² + 228.795146669203 x + 3.49481200157248
1030.00
830.00
630.00
430.00
230.00
30.00
0 2 4 6 8 10 12 14
Penurunan (mm)

x y ln(x) (ln(x))^2 ln(x).y


0.33 38.6 -1.11 1.23 -42.75
0.64 96.4 -0.45 0.21 -43.78
1.27 260.3 0.24 0.06 62.21
1.91 424.1 0.64 0.42 273.35
2.54 607.3 0.93 0.87 566.09
3.81 771.2 1.34 1.79 1031.52
5.08 902.9 1.63 2.64 1467.48
7.62 1028.2 2.03 4.12 2088.05
10.16 1124.6 2.32 5.38 2607.34
12.70 1195.3 2.54 6.46 3037.95
46.05 6448.8 10.11 23.17 11047.45

Beban (lbs) CBR (%)

208.29 6.94
193.05 4.29
BR rata-rata: 5.62

n (ΣLn(x)y) - (ΣLn(x).Σy)
n (Σ (Ln(x))² - (Σ Ln (x))²
10 11047.45 - 10.11 6448.77
10 23.17 - 102.14
45299.08
129.52
349.74
a = y' - bx'
Σy a= 644.88 - 349.74 1.01
n a= 644.88 - 353.47
6448.77 a= 291.41
10
644.88
y= -10,999x2 + 228,8x + 3,4948
Σ ln(x) y= -22.00 x + 228.80
n = 208.29
10.11 = 193.05
10
1.01
Tabel Pemeriksa
Kelompok
Penetrasi (D) Penetrasi (D) Kumulatif
Tumbukan
(cm) (mm) Tumbukan Penetrasi (cm)
0 0 0 0 5 2
1 5 2 20 10 4
2 5 2 20 15 6
3 5 6 60 20 12
4 5 9 90 25 21
5 5 11 110 30 32
6 5 14 140 35 46
7 5 15 150 40 61
8 5 13 130 45 74
9 5 11 110 50 85
10 5 9 90 55 94
11 5 6 60 60 100
980

120 100
105.44
105 90
80
90

Kumulatif Penetrasi (cm)


70
75
CBR Konus 60

60
60 50

45 40
30
30 24.92
14.63 20
11.24 9.03 8.19 7.48
15 7.48 10
0 2
0 0
0 0.5 1 1.5 2 2.5 3 3.5 0 1
DCP (cm/tumbukan)
Tabel Pemeriksaan DCP
Kelompok 2
DCP DCP CBR
(cm/Tumbukan) (mm/Tumbukan) Konus 60° D*CBR*1/3 CBR DESAIN
0 0 0
0.4 4 105.44 18.90
0.4 4 105.44 18.90
1.2 12 24.92 35.05
1.8 18 14.63 44.03
2.2 22 11.24 49.29
14.63
2.8 28 8.19 56.44
3 30 7.48 58.68
2.6 26 9.03 54.14
2.2 22 11.24 49.29
1.8 18 14.63 44.03
1.2 12 7.48 428.73

7.48
100 94
90 85

80 74
Kumulatif Penetrasi (cm)

70
61
60
50 46

40 32
30
21
20 12
10 4 6
2
0
0 10 20 30 40 50 60
Kumulatif Tumbukan

Anda mungkin juga menyukai