RENCANA CAMPURAN BERASPAL PANAS AC- WC (COMBINED II)
Tanggal Test : 14/09/2021
SIEVE SIZE 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 #100 #200
100.00 100.00 100.00100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Abu batu 53% 53 53 53 53.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Aggregat 0,5 - 1 30% 30 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 100.00 41.59 21.15 7.06 3.08 #REF! #REF! #REF! #REF! 0.00
Aggregat 1 - 2 17% 17 17.00 7.07 3.60 1.20 0.52 #REF! #REF! #REF! #REF! 0.00

Kombinasi 100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Fuller 0.0%
Restriction zones
Spesifikasi 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9
UNIFIELD SOILS CLASIFICATIONS SYSTEM
Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
200 100 50 40 30 16 10 8 4 3/8" 1/2" 3/4" 1" 1.5" 2" 2.5" 3"

100
% Persen Berat Lolos

90

80

70

60

50

40

30

20

10

0
0.01 0.075 0.1 0.15 0.3 0.42 0.6 1 1.18 2 2.36 4.75 9.5 10 12.5 19 25 38 50 63 75
100

Ukuran Saringan (mm)

Diuji Oleh ,

(Agus Saputra)
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

DESIGN MIX FORMULA


AC-WEARING COARSE
(AC-WC)
Kontraktor : PT. Sukma Perkasa Abadi
Tanggal : 08/07/2021 Pekerjaan Rekonstruksi / Peningkatan
Kapasitas Struktur Jalan Ruas Jalan
Sp. Tegal Sari - Tulung Agung (Jalan Rajawali)
I. KOMPOSISI CAMPURAN Kode Paket (BM-DAK-06)
NO COLD BIN MATERIAL
2 Abu Batu : 51.00 %
3 Split 0,5 - 1 : 27.00 %
4 Split 10 - 20 : 20.00 %
5 Aspal : 6.10 %

II. PEKERJAAN MARSHALL


NO PROPERTIES TEST HASIL SPESIFIKASI
1 Penyerapan Aspal % 0.277 Max.1.2
2 Kadar Aspal Optimum % 6.100 -
3 Rongga Terhadap Aggregate % 17.20 Min 15
4 Rongga Terisi Aspal % 74.90 Min. 65
5 Rongga Terhadap Campuran % 4.32 3.0 - 5,0
6 Stability kg 933.65 Min.800
7 Kelelehan / Flow mm 3.47 2-4
8 Marshall Quotient kg/mm 269.31
9 PRD % 2.90 Min 2,0
10 Berat Isi Benda Uji gr/cc 2.254 -
11 Stability Setelah Perendaman 24 Jam Suhu 60 °C % 90.82 Min. 90

III. ANALISA SARINGAN


NO NO SARINGAN 1,5" 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 100 #200
1 COLD BIND 100.0 100.0 100.00 97.08 84.24 57.76 40.35 25.74 19.06 15.31 9.16 5.46
2 SPESIFIKASI 100.0 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9

CATATAN :

Diuji Oleh : Diperiksa Oleh :

Ozy Maulana RUSTAM,S.T


Kegiatan Praktikum Mahasiswa Perencanaan Campuran Hot mix
Universitas Sang Bumi Ruwa Jurai Laston Asphalt Concrette Wearing Coarse
Bandar Lampung

OPTIMUM ASPHALT CONTENT ESTIMATION


AC WEARING FOR QUARRY TANJUNGAN
Date : 19/06/2021

GRADATION COMBINED (% PASSING)


PROPORTION
1.5" 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 100 #200
I CA = 56,26%
FA = 39,30% 100 98.93 90.87 85.92 68.66 43.74 25.32 15.42 11.19 7.0 4.44
FF = 4,44%
II CA = 59,93%
FA = 39,57% 100 99.26 93.72 90.32 68.80 40.07 21.55 11.58 7.31 3.08 0.50
FF = 0,5 %

Calculation
I Asphalt Content proportion I = 0.035 x (%CA) + 0.045 x (%FA) + 0.18 x (%FF) + 1,3
= 0.035 x 56,26 + 0.045 x 39,30 + 0.18 x 4,44 + 1,3
= 5.82 %

II Asphalt Content proportion II = 0.035 x (%CA) + 0.045 x (%FA) + 0.18 x (%FF) + 1,3
= 0.035 x 59,93 + 0.045 x 39,57 + 0.18 x 0,5 + 1,3
= 5.30 %

III Asphalt Content proportion III


= 0.035 x (%CA) + 0.045 x (%FA) + 0.18 x (%FF) + 1,0
= 0.035 x 68,58 + 0.045 x 26,20 + 0.18 x 5,22 + 1,0
= 5.8 %

Tested by Checked by Signed by

643031821.xls Estimasi KAO AC-WC


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151
RENCANA CAMPURAN BERASPAL PANAS AC- WC
Tanggal Test : 19/06/2021
SIEVE SIZE 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 #100 #200
100.00 100.00 100.00100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Abu batu 52% 52 52 52 52.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Aggregat 0,5 - 1 37% 37 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 100.00 41.59 21.15 7.06 3.08 #REF! #REF! #REF! #REF! 0.00
Aggregat 1 - 2 11% 11 11.00 4.57 2.33 0.78 0.34 #REF! #REF! #REF! #REF! 0.00

Kombinasi 100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Fuller
Restriction zones
Spesifikasi 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9
UNIFIELD SOILS CLASIFICATIONS SYSTEM
Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
200 100 50 40 30 16 10 8 4 3/8" 1/2" 3/4" 1" 1.5" 2" 2.5" 3"

100
% Persen Berat Lolos

90

80

70

60

50

40

30

20

10

0
0.01 0.075 0.1 0.15 0.3 0.42 0.6 1 1.18 2 2.36 4.75 9.5 10 12.5 19 25 38 50 63 75
100

Ukuran Saringan (mm)

Diuji Oleh ,

(Agus Saputra)
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

COMBINED SPECIFIC GRAVITY & ABSORPTION FOR AC -WEARING COARSE


(COMPOSITION II)

Date : 5/24/2021

Combined of Bulk Sp. Gr. = 100 = #REF! gr/cc


50 29 21
+ + + +
2.557 #REF! #REF!

Combined of Apparent = 100 = #REF! gr/cc


+ 50 + 29 + 21
+
2.701 #REF! #REF!

Combined of Absorption = 100 = #REF! gr/cc


+ 50 + 29 + 21
2.082 #REF! #REF!

Diuji Oleh ,

(Agus Saputra)

643031821.xls Comb.Spgr (3)


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151
RENCANA CAMPURAN BERASPAL PANAS AC- WC
Tanggal Test : 21/05/2021
SIEVE SIZE 1" 3/4" 1/2"3/8" #4 #8 #16 #30 #50 #100 #200
100.00 100.00 100.00
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Abu batu 50% 50 50 50 50.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Aggregat 0,5 - 1 29% 29 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 100.00 41.59 21.15 7.06 3.08 #REF! #REF! #REF! #REF! 0.00
Aggregat 1 - 2 21% 21 21.00 8.73 4.44 1.48 0.65 #REF! #REF! #REF! #REF! 0.00

Kombinasi 100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Fuller
Restriction zones
Spesifikasi 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9
UNIFIELD SOILS CLASIFICATIONS SYSTEM
Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
200 100 50 40 30 16 10 8 4 3/8" 1/2" 3/4" 1" 1.5" 2" 2.5" 3"

100
% Persen Berat Lolos

90

80

70

60

50

40

30

20

10

0
0.075 0.15 0.3 0.42 0.6 25 75
0.01 0.1 1 1.18 2 2.36 4.75 9.5 10 12.5 19 38 50 63 100

Ukuran Saringan (mm)

Diuji Oleh ,

(Agus Saputra)
MBINED AGGREGATE GRADING TES
T CONCRETTE WEARING COARSE
PERTIES TEST MARSHALL STABILI
T CONCRETTE WEARING COARSE
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151
RENCANA CAMPURAN BERASPAL PANAS AC- WC
Tanggal Test : 7/07/2020
SIEVE SIZE 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 #100 #200
100.00 100.00 100.00
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Abu batu 52% 52 52 52 52.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Aggregat 0,5 - 1 23% 23 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
100.00 100.00 41.59 21.15 7.06 3.08 #REF! #REF! #REF! #REF! 0.00
Aggregat 1 - 2 25% 25 25.00 10.40 5.29 1.77 0.77 #REF! #REF! #REF! #REF! 0.00

Kombinasi 100.00 #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF! #REF!
Fuller
Restriction zones
Spesifikasi 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9
UNIFIELD SOILS CLASIFICATIONS SYSTEM
Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
200 100 50 40 30 16 10 8 4 3/8" 1/2" 3/4" 1" 1.5" 2" 2.5" 3"

100
% Persen Berat Lolos

90

80

70

60

50

40

30

20

10

0
0.075 0.15 0.3 0.42 0.6 25 75
0.01 0.1 1 1.18 2 2.36 4.75 9.5 10 12.5 19 38 50 63 100

Ukuran Saringan (mm)


PLOT CHART TEST MARSHALL
SURAT PENGANTAR
SUMMARY TEST
T CONCRETTE WEARING COARSE
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Pagar Alam No. 257, Langkapura, Kota Bandar Lampung 35151 Telp:(0721) 265734 - Fax:(0721)257838

Bandar Lampung, 19 April 2017

Kepada Yth,
Direktur PT. Yoesman Karya
Di -
Bandar Lampung

SURAT PENGANTAR
No. ...........................................................................................

Memperhatikan Surat Permohonan dari PT. Yoesman Karya, Surat Nomor : 028/PT.YK/BDL/2017, Tanggal 05 April 2017.
Perihal Permohonan Uji Laboratorium Design Mix Formula (DMF) Beton Mutu K-250, yang akan digunakan pada pekerjaan
Proyek Pemeliharaan Berkala Jembatan Bts. Prov Bengkulu - Sp. Gunung Kemala, Padang Tambak - Sp. Gunung Kemala,
dengan ini kami sampaikan :

No Uraian Banyaknya Keterangan

Laporan hasil Design Mix Formula (DMF)


1 1 (satu) Set
Beton Mutu K-250

Demikian, untuk dipergunakan seperlunya.

KEPALA LABORATORIUM
TEKNIK SIPIL UNIVERSITAS SABURAI

FERY HENDI JAYA, S.T, M.T.


al 05 April 2017.
n pada pekerjaan
Gunung Kemala,

eterangan

TORIUM
TAS SABURAI

, S.T, M.T.
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Pagar Alam No. 257, Langkapura, Kota Bandar Lampung 35151 Telp:(0721) 265734 - Fax:(0721)257838

Bandar Lampung, 19 April 2017

Kepada Yth,
Direktur PT. Yoesman Karya
Di -
Bandar Lampung

SURAT PENGANTAR
No. ...........................................................................................

Memperhatikan Surat Permohonan dari PT. Yoesman Karya, Surat Nomor : 028/PT.YK/BDL/2017, Tanggal 05 April 2017.
Perihal Permohonan Uji Laboratorium Design Mix Formula (DMF) Asphalt Concrete Wearing Coarse (AC-WC) , yang akan
digunakan pada pekerjaan Proyek Pemeliharaan Berkala Jembatan Bts. Prov Bengkulu - Sp. Gunung Kemala, Padang
Tambak - Sp. Gunung Kemala, dengan ini kami sampaikan :

No Uraian Banyaknya Keterangan

Laporan hasil Design Mix Formula (DMF)


1 1 (satu) Set
Asphalt Concrete Wearing Coarse (AC-WC)

Demikian, untuk dipergunakan seperlunya.

KEPALA LABORATORIUM
TEKNIK SIPIL UNIVERSITAS SABURAI

FERY HENDI JAYA, S.T, M.T.


al 05 April 2017.
WC) , yang akan
Kemala, Padang

eterangan

TORIUM
TAS SABURAI

, S.T, M.T.
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Pagar Alam No. 257, Langkapura, Kota Bandar Lampung 35151 Telp:(0721) 265734 - Fax:(0721)257838

Bandar Lampung, 19 April 2017

Kepada Yth,
Direktur PT. Yoesman Karya
Di -
Bandar Lampung

SURAT PENGANTAR
No. ...........................................................................................

Memperhatikan Surat Permohonan dari PT. Yoesman Karya, Surat Nomor : 028/PT.YK/BDL/2017, Tanggal 05 April 2017.
Perihal Permohonan Uji Laboratorium Design Mix Formula (DMF) Timbunan Pilihan, yang akan digunakan pada pekerjaan
Proyek Pemeliharaan Berkala Jembatan Bts. Prov Bengkulu - Sp. Gunung Kemala, Padang Tambak - Sp. Gunung Kemala,
dengan ini kami sampaikan :

No Uraian Banyaknya Keterangan

Laporan hasil Design Mix Formula (DMF)


1 1 (satu) Set
Timbunan Pilihan

Demikian, untuk dipergunakan seperlunya.

KEPALA LABORATORIUM
TEKNIK SIPIL UNIVERSITAS SABURAI

FERY HENDI JAYA, S.T, M.T.


al 05 April 2017.
pada pekerjaan
Gunung Kemala,

eterangan

TORIUM
TAS SABURAI

, S.T, M.T.
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

DESIGN MIX FORMULA


AC-WEARING COARSE
(AC-WC)
Kontraktor : CV. REJEKI ANUGRAH ABADI
Tanggal : 08/12/2022 Paket Pekerjaan Jasa Konstruksi :
Peningkatan Ruas Jalan Pejambon - Tugu Sari
(050) (Pinjaman Daerah) Kabupaten Pesawaran
I. KOMPOSISI CAMPURAN
NO COLD BIN MATERIAL
2 Abu Batu : 58.00 %
3 Split 0,5 - 1 : 28.00 %
4 Split 10 - 20 : 16.00 %
5 Aspal : 6.00 %

II. PEKERJAAN MARSHALL


NO PROPERTIES TEST HASIL SPESIFIKASI
1 Penyerapan Aspal % 0.292 Max.1.2
2 Kadar Aspal Optimum % 6.000 -
3 Rongga Terhadap Aggregate % 17.38 Min 15
4 Rongga Terisi Aspal % 72.85 Min. 65
5 Rongga Terhadap Campuran % 4.72 3.0 - 5,0
6 Stability kg 1047.97 Min.800
7 Kelelehan / Flow mm 3.53 2-4
8 Marshall Quotient kg/mm 296.62
9 VIM PRD % 3.10 Min 2,0
10 Berat Isi Benda Uji gr/cc 2.262 -
11 Stability Setelah Perendaman 24 Jam Suhu 60 °C % 91.81 Min. 90

III. ANALISA SARINGAN


NO NO SARINGAN 1,5" 1" 3/4" 1/2" 3/8" #4 #8 #16 #30 #50 100 #200
1 COLD BIND 100.0 100.0 102.00 92.65 81.42 55.95 35.65 26.23 20.01 11.58 8.73 6.26
2 SPESIFIKASI 100.0 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9

CATATAN :

Diuji Oleh : Diperiksa Oleh :

Raja Baharsyah, S.T. Rustam,S.T


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PERCOBAAN MARSHALL
SNI 06 - 2489 - 1991

Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse AGGREGAT KOMPOSISI Bulk Apparent
Diuji Tanggal : 07/12/2022 Abu Batu 58.00% 2.557 2.701
Asal Contoh Uji : Quarry Tanjungan Aggregate 0,5 - 1 cm 28.00% 2.595 2.739
Aggregate 1 - 2 cm 16.00% 2.595 2.739

Spec. % Aspal VOLUME BERAT BERAT % VOLUME % VOLUME % RONGGA % RONGGA % RONGGA KELELEHAN MARSHALL PENYERAPAN
BERAT (Gram) STABILITY ( KG)
No Terhadap Campuran ISI JENIS ASPAL AGGREGAT TERHADAP DALAM TERISI (mm) QUOTIEN ASPAL
DI UDARA DI AIR SSD MAKSIMUM (dgn BJ Eff.) AGGREGAT CAMPURAN ASPAL DIAL MEAN ADJUST kg/mm
A B C D E F G H I J L M N O P Q R S
% Bit by % Bit by Dari Dari Dari C 100 BxG (100-B)xG 100-(100-B)G 100 - (100xG) Dari Dari Dari Dari Q B+T(100-B)
WT of WT of Lab. Lab. Lab. E-D F 100-B B (t) (y) (x) H (L-M)
/L x 100 Lab. Lab. Lab. Lab. R x
Agg mix (y) (t) - 100T/H
Marshall Stability Soaking 30 Minutes At Temperature 60 ºc
1 6.38 6.00 1198.2 676.5 1207 530.50 2.259 2.374 13.07 82.08 17.28 4.84 71.97 74 1101.6 1057.5 3.60 294 0.292
2 6.38 6.00 1199.5 677.5 1208.6 531.10 2.259 2.374 13.07 82.08 17.28 4.84 71.97 74 1101.6 1057.5 3.50 302 0.292
3 6.38 6.00 1196.6 678.2 1205.9 527.70 2.268 2.374 13.12 82.41 17.59 4.47 74.62 72 1071.8 1028.9 3.50 294 0.292
Average 2.262 2.374 13.09 82.19 17.38 4.72 72.85 73 1091.6 1048.0 3.53 297 0.292

Marshall Stability Soaking 24 Hours At Temperature 60 ºc


1 6.38 6.00 1199.8 677.5 1207.4 529.90 2.264 2.374 13.10 82.26 17.10 4.63 72.89 68 1012.2 971.8 3.30 294 0.292
2 6.38 6.00 1201.3 679.3 1210.5 531.20 2.261 2.374 13.08 82.16 17.21 4.76 72.33 66 982.5 943.2 3.10 304 0.292
3 6.38 6.00 1197.6 676.5 1207 530.50 2.257 2.374 13.06 82.01 17.99 4.93 72.61 68 1012.2 971.8 3.50 278 0.292
Average 2.261 2.374 13.08 82.14 17.43 4.77 72.61 67 1002.3 962.2 3.30 292 0.292

962,2 / 1048,0 x 100 = 91,81 %


Marshall Stability Soaking 24 Hours At Temperature 60 ºc

CORRECTION PR 9:
1
2
3

Diuji Oleh

Catatan : Berat Jenis Aspal n= 1.037 (t)


: Berat Jenis Aggregat Bulk n= 2.567 (x)
: Berat Jenis Aggregate Eff. n= 2.587 (y) Ozy Maulana
: Proving ring = 14.886 KG Teknisi Lab

643031821.xls Ret 30 Mn
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PERCOBAAN MARSHALL
SNI 06 - 2489 - 1991

Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse AGGREGAT KOMPOSISI Bulk Apparent
Diuji Tanggal : 05/12/2022 Abu Batu 58.00% 2.557 2.701
Asal Contoh Uji : Quarry Tanjungan Aggregate 0,5 - 1 cm 28.00% 2.595 2.739
Aggregate 1 - 2 cm 16.00% 2.595 2.739

Spec. % Aspal VOLUME BERAT BERAT % VOLUME % VOLUME % RONGGA % RONGGA % RONGGA KELELEHAN MARSHALL PENYERAPAN
BERAT (Gram) STABILITY ( KG)
No Terhadap Campuran ISI JENIS ASPAL AGGREGAT TERHADAP DALAM TERISI (mm) QUOTIEN ASPAL
DI UDARA DI AIR SSD MAKSIMUM (dgn BJ Eff.) AGGREGAT CAMPURAN ASPAL DIAL MEAN ADJUST kg/mm
A B C D E F G H I J L M N O P Q R S
% Bit by % Bit by Dari Dari Dari C 100 BxG (100-B)xG 100-(100-B)G 100 - (100xG) Dari Dari Dari Dari Q B+T(100-B)
WT of WT of Lab. Lab. Lab. E-D F 100-B B (t) (y) (x) H /L x 100
(L-M) Lab. Lab. Lab. Lab. R x
Agg mix (y) (t) - 100T/H
1 5.82 5.50 1193.2 684.1 1200.8 516.70 2.309 2.390 12.25 84.35 15.00 3.39 77.40
2 5.82 5.50 1199.5 687.6 1206.7 519.10 2.311 2.390 12.26 84.42 14.92 3.31 77.85
3 5.82 5.50 1199.5 687.6 1206.7 519.10 2.311 2.390 12.26 84.42 14.92 3.31 77.85
Average 2.310 2.390 12.25 84.38 14.96 3.35 77.63

1 6.38 6.00 1193.3 684.7 1201.7 517.00 2.308 2.374 13.35 83.86 15.48 2.78 82.05
2 6.38 6.00 1196.6 685.0 1204.4 519.40 2.304 2.374 13.33 83.72 15.63 2.95 81.13
3 6.38 6.00 1199.5 687.6 1206.7 519.10 2.311 2.374 13.37 83.97 15.37 2.65 82.74
Average 2.306 2.374 13.34 83.79 15.56 2.86 81.59

1 6.95 6.50 1190.2 679.5 1197.6 518.10 2.297 2.358 14.40 83.02 16.33 2.59 84.16
2 6.95 6.50 1191.7 681.8 1200.3 518.50 2.298 2.358 14.40 83.06 16.30 2.55 84.39
3 6.95 6.50 1199.5 687.6 1206.7 519.10 2.311 2.358 14.49 83.53 15.83 1.99 87.41
Average 2.298 2.358 14.40 83.04 16.32 2.57 84.27

Percentage Of Refusal density ( VIM PRD)

CORRECTION PR 9:
1
2
3

Diuji Oleh
Catatan : Berat Jenis Aspal n= 1.037 (t)
: Berat Jenis Aggregat Bulk n= 2.567 (x)
: Berat Jenis Aggregate Eff. n= 2.587 (y)
: Proving ring = 14.886 Kg Ozy Maulana
Teknisi Lab

643031821.xls PRD
PENYERAPAN

643031821.xls PRD
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

APPENDIX 7.08.E
PLOT OF MARSHALL TEST
Date : 03/12/2022

Asphalt Content vs Density Asphalt Content ><Stability


Density (gr/k m3)

Stability (km3)
1300
2.290 1200
1050,0 kg
1100
2.275 gr/cc 1000
2.280
900

2.270 `
800
6,00 %
700
600
500
2.260
6,00 %
400
300
2.250
200
100
2.240 0
A s phalt Content (%) As phalt Content (%)
4.50 5.00 5.50 6.00 6.50 7.00 7.50 8.00 4.50 5.00 5.50 6.00 6.50 7.00 7.50 8.00

Asphalt Content ><Flow Asphalt Content ><MQ

6.00 600
MQ (kg/mm)
Flow (mm)

5.00 500
3.30 mm
4.00 400
300,0 mm/kg
3.00 300

6,00 %
2.00 200
6,00 %
1.00 100

0.00 0
Asphalt Content (%) Asphalt Content (%)
4.50 5.00 5.50 6.00 6.50 7.00 7.50 8.00 4.50 5.00 5.50 6.00 6.50 7.00 7.50

Asphalt Content ><VIM


10.00 Asphalt Content ><VMA
Marshall 75 & 2 20.00
8.00 17,10 %
PRD 400 & 2 18.00
4,20 %
VMA (%)
VIM (%)

6.00

16.00

4.00 6,00 %
14.00

2.00 2,80%
6,00 % 12.00

0.00
Asphalt Content (%)
10.00 Asphalt Content (%)
4.50 5.00 5.50 6.00 6.50 7.00 7.50 8.00
4.50 5.00 5.50 6.00 6.50 7.00 7.50 8.00

Mix Property Requirement Asphalt Content


Asphalt Content ><VFB
120.00 5,0 6,0
5.5 6.5 7,0 ,

100.00 Density
78,00 %
VFB (%)

Stability
80.00

Flow
60.00
6,00 % VIM Marshall
40.00
VIM PRD
20.00
VMA
0.00
As phalt Content (%)
VFB
4.00 4.50 5.00 5.50 6.00 6.50 7.00 7.50

Diuji Oleh

Ozy Maulana
Teknisi Lab

643031821.xls Chart Marshall


643031821.xls Chart Marshall
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PERCOBAAN MARSHALL
SNI 06 - 2489 - 1991

Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse AGGREGAT KOMPOSISI Bulk Apparent
Diuji Tanggal : 02/12/2022 Abu Batu 58.00% 2.557 2.701
Asal Contoh Uji : Quarry Tanjungan Aggregate 0,5 - 1 cm 28.00% 2.595 2.739
Aggregate 1 - 2 cm 16.00% 2.595 2.739

Spec. % Aspal VOLUME BERAT BERAT % VOLUME % VOLUME % RONGGA % RONGGA % RONGGA KELELEHAN MARSHALL PENYERAPAN
BERAT (Gram) STABILITY ( KG)
No Terhadap Campuran ISI JENIS ASPAL AGGREGAT TERHADAP DALAM TERISI (mm) QUOTIEN ASPAL
DI UDARA DI AIR SSD MAKSIMUM (dgn BJ Eff.) AGGREGAT CAMPURAN ASPAL DIAL MEAN ADJUST kg/mm
A B C D E F G H I J L M N O P Q R S
% Bit by % Bit by From From From C 100 BxG (100-B)xG 100-(100-B)G 100 - (100xG) From From From From Q B+T(100-B)
WT of WT of Lab. Lab. Lab. E-D F 100-B B (t) (y) (x) H /L x 100
(L-M) Lab. Lab. Lab. Lab. R x
Agg mix (y) (t) - 100T/H
1 6.95 6.50 1194.38 676.18 1202.58 526.40 2.269 2.358 14.22 82.01 17.35 3.77 78.25 63 937.8 900.3 3.1 290 0.294
2 6.95 6.50 1192.88 676.08 1200.48 524.40 2.275 2.358 14.26 82.22 17.14 3.52 79.46 72 1071.8 1028.9 2.9 355 0.294
3 6.95 6.50 1193.48 675.88 1202.18 526.30 2.268 2.358 14.22 81.97 18.03 3.82 78.83 70 1042.0 1000.3 3.6 278 0.294
Average 2.271 2.358 14.23 82.07 17.51 3.70 78.85 68 1017.2 976.5 3.2 308 0.294

1 7.53 7.00 1194.58 675.18 1202.38 527.20 2.266 2.342 15.30 81.46 18.54 3.25 82.50 60 893.2 857.4 3.4 252 0.291
2 7.53 7.00 1191.88 673.88 1200.08 526.20 2.265 2.342 15.29 81.42 18.58 3.29 82.30 63 937.8 900.3 3.9 231 0.291
3 7.53 7.00 1190.58 674.38 1199.38 525.00 2.268 2.342 15.31 81.53 18.47 3.16 82.89 53 789.0 757.4 3.8 199 0.291
Average 2.266 2.342 15.30 81.47 18.53 3.23 82.56 59 873.3 838.4 3.7 227 0.291

CORRECTION PR 9:
1
2
3

Diuji Oleh
Catatan : Berat Jenis Aspal n= 1.037 (t)
: Berat Jenis Aggregat Bulk n= 2.567 (x)
: Berat Jenis Aggregate Eff. n= 2.587 (y)
: Proving ring = 14.886 Kg Ozy Maulana
Teknisi Lab

643031821.xls Marshall % (2)


PENYERAPAN

643031821.xls Marshall % (2)


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PERCOBAAN MARSHALL
SNI 06 - 2489 - 1991

Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse AGGREGAT KOMPOSISI Bulk Apparent
Diuji Tanggal : 02/12/2022 Abu Batu 58.00% 2.557 2.701
Asal Contoh Uji : Quarry Tanjungan Aggregate 0,5 - 1 cm 28.00% 2.595 2.739
Aggregate 1 - 2 cm 16.00% 2.595 2.739

Spec. % Aspal VOLUME BERAT BERAT % VOLUME % VOLUME % RONGGA % RONGGA % RONGGA KELELEHAN MARSHALL PENYERAPAN
BERAT (Gram) STABILITY ( KG)
No Terhadap Campuran ISI JENIS ASPAL AGGREGAT TERHADAP DALAM TERISI (mm) QUOTIEN ASPAL
DI UDARA DI AIR SSD MAKSIMUM (dgn BJ Eff.) AGGREGAT CAMPURAN ASPAL DIAL MEAN ADJUST kg/mm
A B C D E F G H I J L M N O P Q R S
% Bit by % Bit by From From From C 100 BxG (100-B)xG 100-(100-B)G 100 - (100xG) From From From From Q B+T(100-B)
WT of WT of Lab. Lab. Lab. E-D F 100-B B (t) (y) (x) H /L x 100
(L-M) Lab. Lab. Lab. Lab. R x
Agg mix (y) (t) - 100T/H
1 5.26 5.00 1198.09 676.29 1207.29 531.00 2.256 2.407 10.88 82.85 16.51 6.27 62.01 53 789.0 757.4 2.9 259 0.295
2 5.26 5.00 1193.69 676.69 1203.79 527.10 2.265 2.407 10.92 83.18 16.18 5.90 63.53 61 908.0 871.7 2.7 320 0.295
3 5.26 5.00 1197.39 678.09 1205.99 527.90 2.268 2.407 10.94 83.29 16.71 5.78 65.45 66 982.5 943.2 3.4 276 0.295
Average 2.263 2.407 10.91 83.10 16.47 5.98 63.66 60 893.2 857.4 3.0 285 0.295

1 5.82 5.50 1193.49 679.99 1204.69 524.70 2.275 2.390 12.07 83.10 16.90 4.81 71.52 63 937.8 900.3 3.2 280 0.286
2 5.82 5.50 1195.69 679.39 1205.29 525.90 2.274 2.390 12.06 83.07 16.93 4.85 71.34 67 997.4 957.5 3.7 257 0.286
3 5.82 5.50 1196.29 677.79 1204.69 526.90 2.270 2.390 12.04 82.92 17.08 5.02 70.60 74 1101.6 1057.5 3.6 292 0.286
Average 2.273 2.390 12.06 83.03 16.97 4.90 71.15 68 1012.2 971.8 3.5 276 0.286

1 6.38 6.00 1193.29 679.49 1203.49 524.00 2.277 2.374 13.18 82.74 17.26 4.09 76.33 77 1146.2 1100.4 3.5 313 0.292
2 6.38 6.00 1192.79 676.79 1200.99 524.20 2.275 2.374 13.16 82.66 17.34 4.17 75.95 79 1176.0 1129.0 3.7 303 0.292
3 6.38 6.00 1191.09 675.69 1198.69 523.00 2.277 2.374 13.18 82.74 17.26 4.09 76.33 71 1056.9 1014.6 3.7 273 0.292
Average 2.276 2.374 13.17 82.71 17.29 4.11 76.20 76 1126.4 1081.3 3.7 296 0.292

CORRECTION PR 9:
1
2
3

Diuji Oleh
Catatan : Berat Jenis Aspal n= 1.037 (t)
: Berat Jenis Aggregat Bulk n= 2.567 (x)
: Berat Jenis Aggregate Eff. n= 2.587 (y)
: Proving ring = 14.886 Kg Ozy Maulana
Teknisi Lab

643031821.xls Marshall 4 %
PENYERAPAN

643031821.xls Marshall 4 %
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PERHITUNGAN BERAT JENIS EFEKTIF


& BERAT JENIS MAKSIMUM AC WEARING COARSE

Date : 29/11/2022

Hasil Uji max. Berat Jenis dari campuran pada kadar aspal optimum (6,00 %) = 2.374 gr/cc

Berat Jenis Aggregate Efektif = 100 - 6.00


100 6.00 = 2.587 gr/cc
-
2.374 1.037

Berat Jenis maksimum :

II. Aspal 5,00 % = 100


100 - 5,00 5 = 2.407 gr/cc
+
2.587 1.037

III. Aspal 5,5% = 100


100 - 5,5 5.50 = 2.390 gr/cc
+
2.587 1.037

IV. Aspal 6,00 % = 100


100 - 6,00 6.00 = 2.374 gr/cc
+
2.587 1.037

V. Aspal 6,5% = 100


100 - 6.5 6.50 = 2.358 gr/cc
+
2.587 1.037

VI. Aspal 7,00 % = 100


100 - 7,00 7.00 = 2.342 gr/cc
+
2.587 1.037

Diuji Oleh

Agus Saputra
Teknisi Lab
643031821.xls Cal. GMM
643031821.xls Cal. GMM
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No.468, Kota Bandar Lampung 35151

MAXIMUM SPESIFIC GRAVITY OF MIX (GMM)

Type of mix : Design Mix Formula AC Wearing Coarse

Date of Test : 28/11/2022

No Description Unit
I II I II I II I II

1 Weight of Pan + sample A gr 1450.0 1468.5


2 Weight of Pan B gr 266.8 271.1
3 Weight of sample C=A-B gr 1183.2 1197.4

4 Weight of flask + water D gr 4953.5 4953.5

5 Weight of flask + water + sample F gr 5642.1 5642.8

6 Max Sp. Gr. G=C/((C-D)-F) gr/cc 2.392 2.357

7 Temperature of sample C 30 30 29 29 29 29 29 29

8 Correction of temperature 0.9957 0.9957 0.996 0.996 0.996 0.996 0.996 0.996

9 GMM gr/cc 2.392 2.357


10 Average 2.374

Remarks : Asphalt Content 6.00%

Diuji Oleh

Agus Saputra
Teknisi Lab

643031821.xls GMM Test


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PEMERIKSAAN BERAT JENIS AGGREGAT KASAR


SNI 1969:2008

Kontraktor : PT. Yoesman Karya


Jenis Contoh Uji : Pasir
Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse
Diuji Tanggal : 25/09/2019
Asal Contoh Uji : Quarry Teluk Semaka
Aggregate Tertahan #4
No Contoh I II
Berat Benda Uji Kering Open BK
Berat Benda Uji Kering Perm. Jenuh BJ
Berat Benda Uji Didalam Air BA
BK
Berat jenis (Bulk)
BJ - BA Rata-rata
BJ
Berat Jenis Kering Permukaan Jenuh
BJ - BA Rata-rata
BK
Berat Jenis Semu (Apparent)
BK - BA Rata-rata
BJ - BK
Penyerapan (absorption) X 100 %
BK Rata-rata

PEMERIKSAAN BERAT JENIS AGGREGAT HALUS


SNI 1969:2008

Aggregate Lewat #4
No. Contoh I II
Berat Benda Uji Kering Perm. Jenuh (SSD) 500 500.00 500.00
Berat Benda Uji Kering Open BK 487.20 487.50
Berat Picnometer diisi Air (25%c) B 669.50 689.50
Berat Picnometer
+Berat Uji (SSD) Bt 976.50 997.40
+air (25%)
BK 2.524 2.538
Berat jenis (Bulk)
(B + 500 - Bt) Rata-rata 2.531
500 2.591 2.603
Berat Jenis Kering Permukaan Jenuh
(B + 500 - Bt) Rata-rata 2.597
BK 2.704 2.714
Berat Jenis Semu (Apparent)
(B + BK - Bt) Rata-rata 2.709
500 - BK 2.627 2.564
Penyerapan (absorption) X 100 %
BK Rata-rata 2.596

Remarks :

643031821.xls spgr PASIR NEW (2)


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

COMBINED SPECIFIC GRAVITY & ABSORPTION FOR AC -WEARING COARSE


(COMPOSITION I)

Date : 2/7/2022

Combined of Bulk Sp. Gr. = 100 = 2.567 gr/cc


58 28 16
+ + + +
2.557 2.595 2.595

Combined of Apparent = 100 = 2.664 gr/cc


+ 58 + 28 + 16
+
2.701 2.739 2.739

Combined of Absorption = 100 = 2.014 gr/cc


+ 58 + 28 + 16
2.082 2.018 2.018

Diuji Oleh

Agus Saputra
Teknisi Lab

643031821.xls Comb.Spgr (2)


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

SPECIFIC GRAVITY AND ABSORPTION TEST


AASHTO : T- 85 & 84

Source of Sample : Fine Aggregate / Pasir


Discription : Passing # 4
To be Use for : Design Mix Formula AC Binder Coarse
Date of Test : 24/09/2019
Sample from : Quarry PT. SBSL Tanjungan

Aggregate Retained #4
No.sample I II
Weight of Dry Sample (gr) A
Weight of Sample SSD (gr) B
Weight of Sample in water (gr) C

Bulk of Spesific Gravity (gr/cm3) A


B-C Average :

Bulk of Spesific Gravity SSD (gr/cm3) B


B-C Average :

Apparent Sp. Gravity (gr/cm3) A


A-C Average :

Absorption (%) B - A *100%


A Average :

Aggregate Passing #4
No.sample I II
Weight of Dry Sample (gr) A 488.20 488.70
Weight of Picnometer+Water (gr) B 668.20 690.60
Weight of Sample+Picn.+Water (gr) C 980.10 992.50
A 2.595 2.467
Bulk of Spesific Gravity (gr/cm3)
B + 500 - C Average : 2.531
500 2.658 2.524
Bulk of Spesific Gravity SSD (gr/cm3)
B + 500 - C Average : 2.591
A 2.769 2.616
Apparent Sp. Gravity (gr/cm3)
B+A - C Average : 2.693
500 - A *100% 2.417 2.312
Absorption (%)
A Average : 2.365

Remarks :

643031821.xls spgr Pasir


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

SPECIFIC GRAVITY AND ABSORPTION TEST


AASHTO : T- 85 & 84
To be Use for : Design Mix Formula AC Wearing Coarse
Date of Test : 25/11/2022
Sample from : Quarry Tanjungan
Material : Fine Aggregate / Abu batu
Aggregate Passing #4
No.sample I II
Weight of Dry Sample (gr) A 489.65 489.95
Weight of Picnometer+Water (gr) B 684.55 686.35
Weight of Sample+Picn.+Water (gr) C 993.15 994.65
A 2.558 2.556
Bulk of Spesific Gravity (gr/cm3)
B + 500 - C Average : 2.557
500 2.612 2.608
Bulk of Spesific Gravity SSD (gr/cm3)
B + 500 - C Average : 2.610
A 2.705 2.697
Apparent Sp. Gravity (gr/cm3)
B+A - C Average : 2.701
500 - A *100% 2.114 2.051
Absorption (%)
A Average : 2.082

Material : Medium Aggregate 5/10 mm


Aggregate Retained #4
No.sample I II
Weight of Dry Sample (gr) A 1890.85 1895.35
Weight of Sample SSD (gr) B 1929.05 1933.55
Weight of Sample in water (gr) C 1201.55 1202.15
A 2.599 2.591
Bulk of Spesific Gravity (gr/cm3)
B-C Average : 2.595
B 2.652 2.644
Bulk of Spesific Gravity SSD (gr/cm3)
B-C Average : 2.691
A 2.743 2.734
Apparent Sp. Gravity (gr/cm3)
A-C Average : 2.739
B - A *100% 2.020 2.015
Absorption (%)
A Average : 2.018

Material : Medium Aggregate 10/20 mm


Aggregate Retained #4
No.sample I II
Weight of Dry Sample (gr) A 1890.85 1895.35
Weight of Sample SSD (gr) B 1929.05 1933.55
Weight of Sample in water (gr) C 1201.55 1202.15
A 2.599 2.591
Bulk of Spesific Gravity (gr/cm3)
B-C Average : 2.595
B 2.652 2.644
Bulk of Spesific Gravity SSD (gr/cm3)
B-C Average : 2.691
A 2.743 2.734
Apparent Sp. Gravity (gr/cm3)
A-C Average : 2.739
B - A *100% 2.020 2.015
Absorption (%)
A Average : 2.018

Diuji Oleh

643031821.xls spgr Abu batu


Agus Saputra
Teknisi Lab

643031821.xls spgr Abu batu


UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PENGUJIAN KEAUSAN (ABRASION) UNTUK AGREGAT KASAR


DENGAN MENGGUNAKAN MESIN LOS ANGELES

Kontraktor : CV. Dwi Cendikia


Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse

Asal Contoh Uji : Tanjungan

UKURAN SARINGAN (mm) INDIKASI UKURAN BERAT (Gram) INDIKASI UKURAN BERAT (Gram)
Sampel A Sampel B
LOLOS TERTAHAN SEBELUM SEBELUM
76.20 63.50
63.50 50.80
50.80 37.50
37.50 25.40
25.40 19.00 2,500 2,500
19.00 12.50 2,500 2,500
12.50 9.50
9.50 6.30
6.30 4.75
4.75 2.36
Berat Total contoh 5,000 5,000
Sebelum diuji (A)
Berat Contoh Tertahan 4,138.0 4,137.0
Pada Saringan 1.18 mm (B)
KEAUSAN (ABRASI) 17.24 17.26
(A - B) / A x 100%

RATA-RATA (%) 17.25

Keterangan :
Dipakai Gradasi B ( 500 putaran, 11 bola baja )
Didapat keausan agregat kasar sebesar :
= 17.25%
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151
RENCANA CAMPURAN BERASPAL PANAS AC- WC (COMBINED I)
Tanggal Test :24/11/2022
SIEVE SIZE 1" 3/4" 1/2"3/8" #4 #8 #16 #30 #50 #100 #200
100.00 100.00 100.00
100.00 76.64 58.60 44.07 33.60 19.11 14.26 10.08
Abu batu 58% 58 58 58 58.00 44.45 33.99 25.56 19.49 11.09 8.27 5.84
100.00 100.00 100.00 71.55 37.02 4.16 2.41 1.89 1.76 1.64 1.50
Aggregat 0,5 - 1 28% 28 28.00 28.00 20.03 10.37 1.16 0.68 0.53 0.49 0.46 0.42
100.00 100.00 41.59 21.15 7.06 3.08 0.00 0.00 0.00 0.00 0.00
Aggregat 1 - 2 16% 16 16.00 6.65 3.38 1.13 0.49 0.00 0.00 0.00 0.00 0.00

Kombinasi 102.00 102.00 92.65 81.42 55.95 35.65 26.23 20.01 11.58 8.73 6.26
Fuller 0.0%
Restriction zones
Spesifikasi 100 100 90-100 77-90 53-69 33-53 21-40 14-30 9-22 6-15 4-9
UNIFIELD SOILS CLASIFICATIONS SYSTEM
Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
200 100 50 40 30 16 10 8 4 3/8" 1/2" 3/4" 1" 1.5" 2" 2.5" 3"

100
% Persen Berat Lolos

90

80

70

60

50

40

30

20

10

0
0.075 0.15 0.3 0.42 0.6 25 75
0.01 0.1 1 1.18 2 2.36 4.75 9.5 10 12.5 19 38 50 63 100

Ukuran Saringan (mm)

Diuji Oleh ,

Agus Saputra
Teknisi Lab
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PENGUJIAN ANALISA SARINGAN

Jenis Contoh Uji : Split 10 - 20 mm


Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse
Diuji Tanggal : 24/11/2022
Asal Contoh Uji : Quarry Tanjungan

Berat Bahan Kering (1) : 1915.2 gr


Berat Bahan Kering (2) : 1832.2 gr

Berat Jumlah berat JUMLAH PERSEN


Saringan tertahan Tertahan Tertahan Lewat Rata - Rata
(gr) (gr) (%) (%)

No. (mm) 1 2 1 2 1 2 1 2 (%)

3/4" 19.050 0 0 0.00 0.00 100.00 100.00 100.00

1/2" 12.700 1078.5 1108.6 56.31 60.51 43.69 39.49 41.59

3/8" 9.530 1466.5 1486.5 76.57 81.13 23.43 18.87 21.15

#4 4.750 1765.4 1716.8 92.18 93.70 7.82 6.30 7.06

#8 2.360 1850 1781.6 96.60 97.24 3.40 2.76 3.08

Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
20 10 50 4 3 16 10 8 4 3/8" 1/2 3/4 1" 1.5 2" 2.5" 3"
0 0 0 0 " " "
% Persen Berat Lolos

100.00

90.00

80.00

70.00

60.00

50.00

40.00

30.00

20.00

10.00

0.00
0.0 0.1 0.3 0.4 0.6 1.18 2 2.36 25 63 7
0.010 0.100 1.000 4.75 10.00012.5
9.5 19 38 50 100.000
75 5 2 5

Ukuran Saringan (mm)

Diuji Oleh,

Agus Saputra
Teknisi Lab
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PENGUJIAN ANALISA SARINGAN

Jenis Contoh Uji : Split 05 - 10 mm


Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse
Diuji Tanggal : 24/11/2022
Asal Contoh Uji : Quarry Tanjungan

Berat Bahan Kering (1) : 1568.5 gr


Berat Bahan Kering (2) : 1559.5 gr

Berat Jumlah berat JUMLAH PERSEN


Saringan tertahan Tertahan Tertahan Lewat Rata - Rata
(gr) (gr) (%) (%)

No. (mm) 1 2 1 2 1 2 1 2 (%)

3/4" 19.050 0 0 0.00 0.00 100.00 100.00 100.00

3/8" 9.530 466.5 423.5 29.74 27.16 70.26 72.84 71.55

#4 4.750 1023 947.1 65.22 60.73 34.78 39.27 37.02

#8 2.360 1505 1492.9 95.95 95.73 4.05 4.27 4.16

#16 1.180 1531.7 1520.8 97.65 97.52 2.35 2.48 2.41

#30 0.600 1540.1 1528.9 98.19 98.04 1.81 1.96 1.89

#50 0.300 1541.7 1531.1 98.29 98.18 1.71 1.82 1.76

#100 0.150 1545 1531.6 98.50 98.21 1.50 1.79 1.64

#200 0.075 1546.8 1534.3 98.62 98.38 1.38 1.62 1.50

Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
20 10 50 4 3 16 10 8 4 3/8" 1/2 3/4 1" 1.5 2" 2.5" 3"
0 0 0 0 " " "
% Persen Berat Lolos

100.00

90.00

80.00

70.00

60.00

50.00

40.00

30.00

20.00

10.00

0.00
0.0 0.1 0.3 0.4 0.6 1.18 2 2.36 25 63 7
0.010 0.100 1.000 4.75 10.00012.5
9.5 19 38 50 100.000
75 5 2 5

Ukuran Saringan (mm)

Diuji Oleh,

Agus Saputra
Teknisi Lab
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PENGUJIAN ANALISA SARINGAN

Jenis Contoh Uji : Abu Batu


Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse
Diuji Tanggal : 24/11/2022
Asal Contoh Uji : Quarry Tanjungan

Berat Bahan Kering (1) : 1593.4 gr


Berat Bahan Kering (2) : 1533.6 gr

Berat Jumlah berat JUMLAH PERSEN


Saringan tertahan Tertahan Tertahan Lewat Rata - Rata
(gr) (gr) (%) (%)

No. (mm) 1 2 1 2 1 2 1 2 (%)

3/4" 19.050 0 0 0.00 0.00 100.00 100.00 100.00

3/8" 9.530 0 0 0.00 0.00 100.00 100.00 100.00

1/4" 6.350 0 0 0.00 0.00 100.00 100.00 100.00

#4 4.750 352.3 377.4 22.11 24.61 77.89 75.39 76.64

#8 2.360 641.1 652.7 40.23 42.56 59.77 57.44 58.60

#16 1.180 895.6 853.6 56.21 55.66 43.79 44.34 44.07

#30 0.600 1053.5 1022.8 66.12 66.69 33.88 33.31 33.60

#50 0.300 1308.9 1221.2 82.15 79.63 17.85 20.37 19.11

#100 0.150 1370.1 1311.2 85.99 85.50 14.01 14.50 14.26

#200 0.075 1436 1376 90.12 89.72 9.88 10.28 10.08

Silt Fine Sand Medium sand Coarse Sand Fine Gravel Coarse Gravel
20 10 50 4 3 16 10 8 4 3/8" 1/2 3/4 1" 1.5 2" 2.5" 3"
0 0 0 0 " " "
% Persen Berat Lolos

100.00

90.00

80.00

70.00

60.00

50.00

40.00

30.00

20.00

10.00

0.00
0.0 0.1 0.3 0.4 0.6 1.18 2 2.36 25 63 7
0.010 0.100 1.000 4.75 10.00012.5
9.5 19 38 50 100.000
75 5 2 5

Ukuran Saringan (mm)

Diuji Oleh,

Agus Saputra
Teknisi Lab
UNIVERSITAS SANG BUMI RUWA JURAI
LABORATORIUM TEKNIK SIPIL
FAKULTAS TEKNIK JURUSAN TEKNIK SIPIL
Jl. Imam Bonjol No. 468 , Langkapura, Kota Bandar Lampung 35151

PENGUJIAN ANALISA SARINGAN

Jenis Contoh Uji : Pasir


Jenis Pekerjaan : Design Mix Formula AC Wearing Coarse
Diuji Tanggal : 23/09/2019
Asal Contoh Uji : Quarry Tanjungan

Berat Bahan Kering (1) : 1055.6 gr


Berat Bahan Kering (2) : 1050.2 gr

Berat Jumlah berat JUMLAH PERSEN


Saringan tertahan Tertahan Tertahan Lewat Rata - Rata
(gr) (gr) (%) (%)

No. (mm) 1 2 1 2 1 2 1 2 (%)

2½" 63.500

2" 50.800

1½" 38.100 0 0 0.00 0.00 100.00 100.00 100.00

1" 25.400 0 0 0.00 0.00 100.00 100.00 100.00

3/4" 19.050 0 0 0.00 0.00 100.00 100.00 100.00

1/2" 12.700 0 0 0.00 0.00 100.00 100.00 100.00

3/8" 9.530 0 0 0.00 0.00 100.00 100.00 100.00

1/4" 6.350

#4 4.750 21.6 29.5 2.05 2.81 97.95 97.19 97.38

#8 2.360 79.5 85.5 7.53 8.14 92.47 91.86 92.01

#10 2.000

#16 1.180 287.2 305.4 27.21 29.08 72.79 70.92 71.39

#30 0.600 567.2 569.2 53.73 54.20 46.27 45.80 45.92

#40 0.425

#50 0.300 736.1 728.1 69.73 69.33 30.27 30.67 30.47

#70 0.212
#100 0.150 928.6 926.2 87.97 88.19 12.03 11.81 11.92
#200 0.075 982.7 974.2 93.09 92.76 6.91 7.24 7.07