Anda di halaman 1dari 46

LABORATORIUM JALAN RAYA

JURUSAN TEKNIK SIPIL


POLITEKNIK NEGERI LHOKSEUMAWE

SUMMARY DESIGN MIX FORMULA


DMF AC - BC
I. KOMPOSISI CAMPURAN AGGREGAT COLD BIN

MATERIAL PROPORSI ( % ) BUKAAN COLD BIN ( cm )

COARSE AGGREGATE COLD BIN I 14.0 % 18.0 % 4.4 cm

MEDIUM AGGREGATE COLD BIN II 36.0 % 34.1 % 7.2 cm

DUST STONE COLD BIN III 25.0 % 23.7 % 5.4 cm

SAND COLD BIN IV 20.0 % 19.0 % 4.4 cm

ASPHALT 5.25 %

TOTAL 95.0 % 100.0 %

III. MARSHALL PROPERTIES

MIX PROPERTIES TEST RESULT REQUIREMENT

PENYERAPAN KADAR ASPAL 3.67 Max. 1.2

RONGGA DALAM CAMPURAN % 39.2 3.5 - 5.5

RONGGA DALAM AGGREGAT % 42.9 Min. 14

RONGGA TERISI ASPAL % 17.8 Min. 63

STABILITAS MARSHALL kg 1129 Min. 800

KELELEHAN mm 3.2 Min. 3

MARSHALL QUOTIENT kg/mm 349.6 Min. 200

STABILITAS MARSHALL SISA % 92.1 Min. 85

RONGGA DALAM CAMPURAN (REFUSAL) % - Min. 2.5

BERAT ISI 2.325

TEMPERATUR MIXING ºc 150 Max. 155º

IV. GRADASI AGGREGATE GABUNGAN


Inc. 1" 3 / 4" 1 / 2" 3 / 8" #4 #8 # 16 # 30 # 50 #100 # 200
UKURAN SARINGAN
mm. 25.4 19 12.7 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075

TOTAL CAMP. 0% 100.0 100.0 90.2 86.7 58.7 30.1 25.0 15.1 10.2 8.1 7.7

MINIMUM 100.0 90 74 64 47 34.6 28.3 20.7 13.7 4 4


SPECT' GRAD.
MAXIMUM 100.0 100 90 82 64 49.0 38 28 20 13 8

FULLER 100.0 87.8 73.2 64.2 47.0 34.3 25.1 18.5 13.6 9.9 7.3
Lampiran Tabel 1.1 Analisa Saringan Agreagat 1"
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC

NAMA PEKERJAAN : ANALISA SARINGAN

LOKASI : LABORATORIUM JALAN RAYA

PELAKSANA : KELOMPOK 2

KELAS : DIV - 3D

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 2 - 11 - 2018
Material : Aggregat 1" Splite
Wt. Sample : 2013 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.0 100.0 25

3/4" 0 0 0.0 100.0

1/2" 1397.2 1397.20 69.4 30.6

3/8" 480.4 1877.60 93.3 6.7

#4 103.1 1980.70 98.4 1.6

#8 12.7 1993.40 99.0 1.0

# 16 1.1 1994.50 99.1 0.9

# 30 0.3 1994.80 99.1 0.9

# 50 0.5 1995.30 99.1 0.9

#100 2.1 1997.40 99.2 0.8

# 200 4.3 2001.70 99.4 0.6

2001.7
TOTAL PASSING ( % )

GRADING CHART
100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0
#200 #50 #30SIEVE#16
SIZE #8 #4 3/8" 1/2" 3/4" 1"
Lampiran Tabel 1.2 Analisa Saringan Agregat 3/8"
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : ANALISA SARINGAN

LOKASI : LABORATORIUM JALAN RAYA


PELAKSANA : KELOMPOK 2

KELAS : DIV - 3D

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 2 - 11 - 2018
Material : Aggregat 3/8" Screen
Wt. Sample : 2220 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0.00 0.0 100.0 11

3/4" 0 0.00 0.0 100.0

1/2" 4.1 4.10 0.2 99.8

3/8" 9.2 13.30 0.6 99.4

#4 1584.2 1597.50 72.0 28.0

#8 554.9 2152.40 97.0 3.0

# 16 24.5 2176.90 98.1 1.9

# 30 0.5 2177.40 98.1 1.9

# 50 0.7 2178.10 98.1 1.9

# 100 9.6 2187.70 98.5 1.5

# 200 7.2 2185.30 98.4 1.6

2194.9
TOTAL PASSING ( % )

GRADING CHART
100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0
#200 #50 #30SIEVE#16
SIZE #8 #4 3/8" 1/2" 3/4" 1"
0.0
Lampiran Tabel 1.3 Analisa Saringan Dust Stone
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : ANALISA SARINGAN
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 2 - 11 - 2018
Material : Dust Stone
Wt. Sample : 2200 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0.00 0.0 100.0 321

3/4" 0 0.00 0.0 100.0

1/2" 0 0.00 0.0 100.0

3/8" 0 0.00 0.0 100.0

#4 141 141.00 6.4 93.6

#8 1715.8 1856.80 84.4 15.6

# 16 212.8 2069.60 94.1 5.9

# 30 17.7 2087.30 94.9 5.1

# 50 0.9 2088.20 94.9 5.1

# 100 6.2 2094.40 95.2 4.8

# 200 11.5 2105.90 95.7 4.3

2105.90
TOTAL PASSING ( % )

GRADING CHART

100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0

0.0 #200 #50 #30SIEVE#16


SIZE #8 #4 3/8" 1/2" 3/4" 1"
Lampiran 1.4 Analisa Saringan Natural Sand
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : ANALISA SARINGAN

LOKASI : LABORATORIUM JALAN RAYA

PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SIEVE ANALISYS
SNI 03-1968-1980
Tanggal Pengujian : 2 - 11 - 2018
Material : Natural Sand
Wt. Sample : 2100 gr

Sieve Indv. Wt. ret. COMULATIVE

Wt. ret Retained Passing SPEC"T


Size ( gr )
( gr ) (%) (%)

1" 0 0 0.0 100.0 375

3/4" 0 0 0.0 100.0

1/2" 0 0 0.0 100.0

3/8" 0 0 0.0 100.0

#4 0 0 0.0 100.0

#8 0.9 0.90 0.0 100.0

# 16 246.8 247.70 11.8 88.2

# 30 1010.1 1257.80 59.9 40.1

# 50 518.5 1776.30 84.6 15.4

# 100 195.9 1972.20 93.9 6.1

# 200 28.1 2000.30 95.3 4.7

2000.3
TOTAL PASSING ( % )

GRADING CHART
100.0

90.0

80.0

70.0

60.0

50.0

40.0

30.0

20.0

10.0
#200 #50 #30SIEVE#16
SIZE #8 #4 3/8" 1/2" 3/4" 1"
0.0
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC

ANALYST AGGREGATE SURFACE AREA


ASTM AGGREGATE GRADING AGGREGATE
COMBINED AGGREGATE GRADING
SIEVE CA MA DS SA SURFACE

SIZE a b c d I II III IV V VI VII VIII IX X XI XII XIII XIV XV XVI XVII XVIII XIX XX XXI FACTOR

1 1/2"

1" 100 100 100 100 95.0

3/4" 100 100 100 100 95.0 100 100 100 100 100 100 100 100 100 100 100 100 100 100
1 x 0.41
1/2" 30.591157 99.815315 100 100 85.2 88.7 85.0 92.5 88.7 85.0 92.5 88.7 85.0 88.7 88.7 88.7 88.7 88.7 88.7

3/8" 6.7262792 99.400901 100 100 81.7 84.8 79.8 89.9 84.8 79.7 89.8 84.8 79.7 84.8 84.8 84.8 84.8 84.8 84.8

#4 1.6 28.040541 93.590909 100 53.7 74.9 68.3 79.7 73.2 66.7 77.8 71.5 65.1 71.3 71.3 71.3 71.3 71.3 71.3 x 0.41

#8 0.9736711 3.045045 15.6 99.957143 25.1 53.1 47.9 46.2 42.1 37.9 34.4 31.4 28.3 31.0 31.0 31.0 31.0 31.0 31.0 x 0.82

# 16 0.9 1.9 5.9272727 88.204762 20.0 44.9 40.5 37.6 34.2 30.8 26.2 24.0 21.6 23.5 23.5 23.5 23.5 23.5 23.5 x 1.64

# 30 0.9041232 1.9189189 5.1227273 40.104762 10.1 21.2 19.2 18.2 16.6 15.1 13.4 12.2 11.1 12.1 12.1 12.1 12.1 12.1 12.1 x 2.87

# 50 0.8792846 1.9 5.1 15.414286 5.2 9.1 8.3 8.4 7.7 7.1 6.9 6.4 5.9 6.3 6.3 6.3 6.3 6.3 6.3 x 6.14

# 100 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 0.0 x 12.29

# 200 0.7749627 1.6 4.8 6.1 3.1 4.4 4.1 4.6 4.2 3.9 4.3 4.0 3.7 4.0 4.0 4.0 4.0 4.0 4.0 x 32.77

Agg. Blend a. Coarse Agg. ( CA ) 14.0 16.2 21.6 10.8 16.2 21.6 10.8 16.2 21.6 16.2 16.2 16.2 16.2 16.2 16.2

ratio b. Medium Agg. ( MA ) 36.0 10.5 12.5 9.9 11.9 13.8 11.5 13.2 15.1 13.5 13.5 13.5 13.5 13.5 13.5

( % by wt. c. Dust Stone ( DS ) 25.0 24.4 21.9 39.6 35.9 32.3 51.8 47.1 42.2 47.2 47.2 47.2 47.2 47.2 47.2

of total agg. d. Sand Agg. ( SA ) 20.0 48.9 43.9 39.6 35.9 32.3 25.9 23.5 21.1 23.0 23.0 23.0 23.0 23.0 23.0

TOTAL AGGREGATE SURFACE AREA 2.8 4.5 4.1 4.3 4.0 3.6 3.7 3.4 3.2 3.4 3.4 3.4 3.4 3.4 3.4
1:2 1:1 2:1 2:1

Remark's :
Lampiran Tabel 1.5 Komposisi Job Mix Formula
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : KOMPOSISI JOB MIX FORMULA
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D
Tanggal : 11/2/2018

KOMPOSISI JOB MIX FORMULA

UKURAN SARINGAN

DATA MATERIAL KOMPOSISI Inc. 1" 3 / 4" 1 / 2" 3 / 8" #4 #8 # 16 # 30 # 50 #100 # 200

mm. 25.4 19 12.7 9.5 4.75 2.36 1.18 0.6 0.3 0.15 0.075
AGG. 1" 14% 100.0 100.0 30.6 6.7 1.6 1.0 0.9 0.9 0.9 0.8 0.6
AGG. 3/8" 36% 100.0 100.0 99.8 99.4 28.0 3.0 1.9 1.9 1.9 1.6 1.6
% Pass. Sive

DUST STONE 25% 100.0 100.0 100.0 100.0 93.6 15.6 5.9 5.1 5.1 4.8 4.3
SAND 20% 100.0 100.0 100.0 100.0 100.0 100.0 88.2 40.1 15.4 6.1 4.7
FILLER 5% 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0 100.0
TOTAL CAMP. 100% 100.0 100.0 90.2 86.7 58.7 30.1 25.0 15.1 10.2 8.1 7.7
MINIMUM 100.0 100.0 90 72 43 28.0 19.0 13 9 6 4
SPECT' GRAD.
MAXIMUM 100.0 100.0 100 90 63 39.1 25.6 19.1 15.5 13 10
FULLER 100.0 87.8 73.2 64.2 47.0 34.3 25.1 18.5 13.6 9.9 7.3

Perkiraan Kadar Aspal Optimum Pb = 0,035 (62,4%) + 0,045 (30,4%) + 0,18 (7,2) + K = (0,5 - 1)
0.035 69.9 0.045 22.0 0.18 8.1 0.6
Pb = 5.5 %

% Kadar Aspal untuk Benda Uji = 5.0 5.5 6.0

GRADING CHART

100
TOTAL % PASSING

Batas Spec Fuller Hasil Gradasi Gabungan


90

80

70

60

50

#200
40

30

20

10

0
#200 #200 #50 #30 #16 #8 #4 3/8" 1/2" 3/4" 1"

SIEVE SIZE
Lampiran Tabel 1.12 Pengujian Berat Jenis Aspal
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : PENGUJIAN BERAT JENIS ASPAL
LOKASI : LABORATORIUM ASPAL
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D
TANGGAL/HARI : 07 NOVEMBER 2018 / RABU

Uraian Berat Satuan


Piknometer kosong + Tutup A 34.98 Gram
Piknometer + Tutup + Air B 64.1 Gram
Piknometer + Tutup + Aspal C 50.21 Gram
Piknometer + Tutup + Aspal + Air D 65.13 Gram
Berat jenis (C-A)/(B-A)-(D-C) 1.07 Gram/ml

Jadi, berat jenis aspal adalah 1,07 gram/ml


JMF LASTON AC-WC (GRADASI KASAR)
Kelompok : 2

Material Persentase
Splite 14%
Screen 36%
Dust 25%
Sand 20%
Filler 5%
Total 100%

Pb 5.5%
4.5% 5% 5.5% 6% 6.5%

Berat Benda Uji = 1200 gram


Pb = 5.5%
Berat Aspal = 1200 x 5,5% 66 gram
Berat Agregat = 1200 - 66 1134 gram
jumlah benda uji 3 buah

Pb = 5,5 %
Material Persentase B.A x Persentase kolom 3 x beda uji
1 2 (1134) x 2 = 3 (3) x 3 = 4
Splite 14% 158.8 476.28
Screen 36% 408.2 1224.72
Dust 25% 283.5 850.5
Sand 20% 226.8 680.4
Filler 5% 56.7 170.1
Total 100% 1134 Pb = 5,5 %
66 gram

Pb = 5 %
Berat Benda Uji = 1200 gram
Pb = 5%
Berat Aspal = 1200 x 5% 60 gram
Berat Agregat = 1200 - 60 1140 gram
jumlah benda uji 3 buah

Pb = 5,5 %
Material Persentase B.A x Persentase kolom 3 x beda uji
1 2 (1140) x 2 = 3 (3) x 3 = 4
Splite 14% 159.6 478.8
Screen 36% 410.4 1231.2
Dust 25% 285.0 855
Sand 20% 228.0 684
Filler 5% 57.0 171
Total 100% 1140 Pb = 5 %
60 gram

Pb = 6 %
Berat Benda Uji = 1200 gram
Pb = 6%
Berat Aspal = 1200 x 6% 72 gram
Berat Agregat = 1200 - 72 1128 gram
jumlah benda uji 3 buah

Pb = 6 %
Material Persentase B.A x Persentase kolom 3 x beda uji
1 2 (1140) x 2 = 3 (3) x 3 = 4
Splite 14% 157.9 473.76
Screen 36% 406.1 1218.24
Dust 25% 282.0 846
Sand 20% 225.6 676.8
Filler 5% 56.4 169.2
Total 100% 1128 Pb = 6 %
72 gram

Rekapitulasi
Splite 14% 476.28 478.8 473.76
Screen 36% 1224.72 1231.2 1218.24
Dust 25% 850.5 855 846
Sand 20% 680.4 684 676.8
Filler 5% 170.1 171 169.2
Total 100% Pb = 5,5 % Pb = 5 % Pb = 6 %
66 gram 60 gram 72 gram
Komulatif
158.8 gram splite
567.0 gram screen
850.5 gram dust
1077.3 gram sand
1134.0 gram filler

Komulatif
159.6 gram splite
570.0 gram screen
855.0 gram dust
1083.0 gram sand
1140.0 gram filler
Komulatif
157.9 gram splite
564.0 gram screen
846.0 gram dust
1071.6 gram sand
1128.0 gram filler

1428.8 gram
3674.2 gram
2551.5 gram
2041.2 gram
510.3 gram
Lampiran Tabel 1.6 Berat Jenis dan Penyerapan Air Agregat Splite
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : BERAT JENIS DAN PENYERAPAN AIR AGREGAT
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SPECIFIC GRAVITY AND ABSORPTION TEST OF COARSE AGGREGATE


SNI 03-1969-1990
Tanggal Pengujian : 3 November 2018
Material : Aggregat 1" Splite

SIZE PARTIKEL

RUN NO.

1 WEIGHT OF ( SSDC + DISH) ( gr ) 1034.60

2 WEIGHT OF DISH ( gr ) 0.00

3 WEIGHT OF SSDC ( gr ) 1-2 1034.60

WEIGHT OF (WIRE BASKET + SSDC)


4 ( gr ) 671.51
IN WATER

5 WEIGHT OF WIRE BASKET IN WATER ( gr ) 0.00

6 WEIGHT OF SSDC IN WATER ( gr ) 4-5 671.51

7 SPGR OF SSDC ( gr ) 3 / (3 - 6) 2.85

AVERAGE 2.85

8 WEIGHT OVEN DRY SAMPLE 984.90

9 BULK SPGR ( gr ) 8 / (3 - 6) 2.71

AVERAGE 2.71

10 VOLUME OF WATER 3-8 49.70

11 APPARENT SPGR ( gr ) 8 / (8 - 6) 3.14

AVERAGE 3.14

12 ABSORPTION PERCENT (%) (10/8) x 100 5.05

AVERAGE 5.05
Lampiran Tabel 1.7 Berat Jenis dan Penyerapan Air Agregat Screen
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : BERAT JENIS DAN PENYERAPAN AIR AGREGAT
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SPECIFIC GRAVITY AND ABSORPTION TEST OF COARSE AGGREGATE


SNI 03-1969-1990
Tanggal Pengujian : 3 November 2018
Material : Aggregat 3/8" Screen

SIZE PARTIKEL

RUN NO.

1 WEIGHT OF ( SSDC + DISH) ( gr ) 1021.80

2 WEIGHT OF DISH ( gr ) 0.00

3 WEIGHT OF SSDC ( gr ) 1-2 1021.80

WEIGHT OF (WIRE BASKET + SSDC)


4 ( gr ) 605.59
IN WATER

5 WEIGHT OF WIRE BASKET IN WATER ( gr ) 0.00

6 WEIGHT OF SSDC IN WATER ( gr ) 4-5 605.59

7 SPGR OF SSDC ( gr ) 3 / (3 - 6) 2.46

AVERAGE 2.46

8 WEIGHT OVEN DRY SAMPLE 972.40

9 BULK SPGR ( gr ) 8 / (3 - 6) 2.34

AVERAGE 2.34

10 VOLUME OF WATER 3-8 49.40

11 APPARENT SPGR ( gr ) 8 / (8 - 6) 2.65

AVERAGE 2.65

12 ABSORPTION PERCENT (%) (10/8) x 100 5.08

AVERAGE 5.08
Lampiran Tabel 1.8 Berat Jenis dan Penyerapan Air Agregat Dust Stone
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : BERAT JENIS DAN PENYERAPAN AIR AGREGAT
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SPECIFIC GRAVITY AND ABSORPTION TEST OF FINE AGGREGATE


SNI 03-1970-1990
Tanggal Pengujian : 3 November 2018
Material : Dust Stone

RUN NO.

NO. OF FLASK

A WEIGHT OF SAMPLE ( S.S.D) ( gr ) 502.4

B WEIGHT OF FLASK + WATER ( gr ) 1287.9

C WEIGHT OF FLASK + WATER + SAMPLE ( gr ) 1675.7

D WEIGHT OF DRY SAMPLE ( gr ) 459.4

1 S.S.D SPGR ( gr ) A/(A+B-C) 4.384

AVERAGE 4.384

2 BULK SPGR ( gr ) D/(A+B-C) 4.009

AVERAGE 4.009

3 APPARENT SPGR ( gr ) D/(B+D-C) 6.417

AVERAGE 6.417

4 ABSORPTION (%) (A-D)/Dx100 9.360

AVERAGE 9.360
Lampiran Tabel 1.9 Berat Jenis dan Penyerapan Air Agregat Sand
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC
NAMA PEKERJAAN : BERAT JENIS DAN PENYERAPAN AIR AGREGAT
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

SPECIFIC GRAVITY AND ABSORPTION TEST OF FINE AGGREGATE


SNI 03-1970-1990
Tanggal Pengujian : 3 November 2018
Material : Sand

RUN NO.

NO. OF FLASK

A WEIGHT OF SAMPLE ( S.S.D) ( gr ) 500.3

B WEIGHT OF FLASK + WATER ( gr ) 1280.5

C WEIGHT OF FLASK + WATER + SAMPLE ( gr ) 1685.8

D WEIGHT OF DRY SAMPLE ( gr ) 489.4

1 S.S.D SPGR ( gr ) A/(A+B-C) 5.264

AVERAGE 5.264

2 BULK SPGR ( gr ) D/(A+B-C) 5.150

AVERAGE 5.150

3 APPARENT SPGR ( gr ) D/(B+D-C) 5.815

AVERAGE 5.815

4 ABSORPTION (%) (A-D)/Dx100 2.221

AVERAGE 2.221
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - BC

NAMA PAKET :

LOKASI :

KONTRAKTOR :

KONSTRUKSI :

ANALISA VOLUMEMERIK

Specific Grafity (kg/cm3)


No Material Percentage (P) Absorbsi (%) Formula
Bulk (Gblk) Apparent (Gap)

1 Agg. 1" 14.0 2.713 3.143 5.046

2 Agg. 3/8" 36.0 2.336 2.651 5.080

3 Dust Stone 25.0 4.009 6.417 9.360

4 Natural Sand 20.0 5.150 5.815 2.221

5 Gs Max of Mixture (Gmm) = 2.430 gr/cm3 AASHTO T 209 pada kadar aspal opt. perkiraan

6 Gs Eff of total Aggregate (Gse) = 4.433 gr/cm3 (100)/(2)/(Gsap)+Gsb/2

7 Gs Bulk of total Aggregate (Gsb) = 3.861 gr/cm3 100/((P1/Gblk1)+(P2/Gblk2)

8 Gs Apparent of tota Aggregate (Gsap) = 5.004 gr/cm3 100/((P1/Gap1)+(P2/Gap2)

9 Gs Bitument (Gb) = 1.100 gr/cm3 AASHTO T 228

10 Absorb. Bitument Content (Pba) = 3.7 % 100*(Gse-Gsb)/(Gsb*Gse)*Gb

11 Opt. Bitument Cont. (estimate) (Pb) = 5.1 % 0.035(%CA)+0.045(%FA)+0.18(%FF)+C

12 Effective Bitument (Pbe) = 1.5 % Pb-(Pba*100-Pb)/100

13 Agg. Surface Area (Asa) = 2.8

14 Bitumen Film Thickness (Bft) = 3.3 micron 1000*(Pb-Pba)/(Asa*(Gb*(100-Pb)))


Lampiran 1.15 Grafik Data Pengujian Marshall
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC


NAMA PEKERJAAN : GRAFIK DATA MARSHALL
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DIV - 3D

GRAFIK DATA MARSHALL


Kepadatan (gr/cm³)

Satabilitas (kg)
Kadar Aspal >< Stabilitas
Kadar Aspal >< Kepadatan

3.00
1320
2.80
2.60 1200
2.40
1080
2.20
2.00 960
1.80
840
1.60
1.40
720
1.20
1.00 600

5.00 5.50 6.00 5.00 5.50 6.00


Kadar Aspal (%) Kadar Aspal (%)

Kadar Aspal >< Marshall quotien


Kadar Aspal >< Kelelehan

8.0 300.00
Flow (%)

M Q (%)

7.0

6.0
200.00
5.0

4.0

3.0 100.00

5.00 5.50 6.00 5.00 5.50 6.00


Kadar Aspal (%) Kadar Aspal (%)

Kadar Aspal >< V I M Kadar Aspal >< V M A

53.00 55.00
V M A (%)
V I M (%)

50.00
46.00
45.00
39.00
40.00

32.00 35.00

25.00 30.00

25.00
18.00
20.00
11.00
15.00

4.00 10.00

5.00 5.50 6.00 5.00 5.50 6.00


Kadar Aspal (%) Kadar Aspal (%)

Kadar Aspal >< V F B

100.00
V F B (%)

80.00

60.00

40.00

20.00

0.00

5.00 5.50 6.00


Kadar Aspal (%)
Lampiran Tabel 1.16 Bart Chart Pengujian Marshall
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE

MIX DESING LASTON AC - WC

NAMA PEKERJAAN : BART CHART

LOKASI : LABORATORIUM JALAN RAYA

PELAKSANA : KELOMPOK 2

KELAS : DIV - 3D

BART CHART

RENTANG KADAR
ASPAL TOTAL
SIFAT - SIFAT CAMPURAN

5.00 5.50 6.00

RONGGA DALAM AGGREGAT (VMA)

RONGGA TERISI ASPAL (VFB)

STABILITAS MARSHALL

KELELEHAN

MARSHALL QUOTIENT

KEPADATAN

RONNGA DALAM CAMPURAN (VIM)

5.3

KADAR ASPAL OPTIMUM = 5,8 %


LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC

NAMA PAKET :

LOKASI :

KONTRAKTOR :

KONSTRUKSI :

BERAT JENIS MAKSIMUM CAMPURAN BERASPAL


SNI 03-6893-2002

NO URAIAN I II

A BERAT BENDA UJI KERING 5525 5648

B BERAT WADAH DALAM AIR 0 0

C BERAT BENDA UJI DALAM AIR 3305 3382

D BERAT JENIS A / A- C 2.489 2.492

F AVERAGE 2.491
Lampiran Tabel 1.13 Data Marshall test
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC
NAMA PEKERJAAN : DATA MARSHALL TEST
LOKASI : LABORATORIUM JALAN RAYA
PELAKSANA : KELOMPOK 2
KELAS : DFIV - 3D

MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 3.861 BJ. EFFECTIVE AGGREGATE ( U ) 4.433 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji Kalibrasi stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm Marshall kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q Q
1 5.00 5.26 1177.50 666.70 1178.88 512 2.299 145 11.338 2016 1828 7.1 256.1
2 1172.80 663.78 1187.80 524 2.238 129 11.338 1793 1602 6.1 262.6
3 1188.90 666.21 1211.35 545 2.181 132 11.338 1835 1569 7.0 223.5
Avg 5.00 5.26 527.113 2.239 3.850 44.9 41.8 13.3 11.338 1667 6.8 247.4
11.338
1 5.50 5.82 1149.60 646.89 1175.49 529 2.175 70 11.338 973 871 8.1 107.5
2 1172.00 661.47 1187.07 526 2.230 120 11.338 1668 1514 6.3 241.1
3 1180.60 667.43 1202.29 535 2.207 135 11.338 1877 1648 7.1 232.2
Avg 5.50 5.82 529.687 2.204 3.800 46.1 42.0 11.9 11.338 1344 7.2 193.6
1 6.00 6.38 1122.00 578.40 1191.72 613 1.829 80 11.338 1112 986 7.5 131.6
2 1124.40 580.70 1141.61 561 2.005 65 11.338 904 835 7.9 105.7
3 1123.40 579.55 1123.57 544 2.065 75 11.338 1043 980 6.7 146.3
Avg 6.00 6.38 572.750 1.966 3.751 52.1 47.6 0.3 11.338 934 7.4 127.9
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 3.861 BJ. EFFECTIVE AGGREGATE ( U ) 4.433 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 6.00 6.00 1064.2 588.4 1051.80 463 2.297 78 1084 984 3.5 281.0
2 1063.4 594.0 1050.50 457 2.329 80 1112 993 3.6 275.9
3 1062.0 591.2 1052.62 461 2.302 79 1098 939 3.6 264.6
Avg 6.00 6.00 460.440 2.309 3.751 43.8 38.4 17.8 972 3.6 273.8

1 6.50 6.50 1053.0 593.6 1047.30 454 2.321 80 1112 995 3.5 284.3
2 1055.4 590.7 1050.50 460 2.295 84 1168 1060 3.6 294.4
3 1052.0 592.2 1048.90 457 2.303 82 1140 1001 4 282.0
Avg 6.50 6.50 456.750 2.306 3.703 44.1 37.7 18.1 1019 3.6 286.9

1 7.00 7.00 1046.0 604.2 1052.50 448 2.333 76 1056 937 3.6 260.2
2 1044.0 596.7 1057.30 461 2.267 78 1084 1002 3.4 294.7
3 1045.0 600.5 1054.90 454 2.299 77 1070 1027 4 293.6
Avg 7.00 7.00 454.450 2.300 3.657 44.6 37.1 18.3 989 3.5 282.8
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

MARSHALL TEST
RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 3.861 BJ. EFFECTIVE AGGREGATE ( U ) 4.433 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 7.00 7.53 1032 590 1027.3 438 2.357 68 945 907 3.3 275.0
2 1028 602 1047.3 445 2.309 66 917 881 3.5 251.6
3 1030 596 1037 442 2.333 67 931 894 3.4 263.0
Avg 7.00 7.53 441.500 2.333 3.657 43.8 36.2 20.0 894 3.4 263.2
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

MARSHALL TEST (STABILITAS SISA)


RSNI M-01-2003

BJ. BULK AGGREGATE ( V ) 3.861 BJ. EFFECTIVE AGGREGATE ( U ) 4.433 BJ. ASPHALT ( T ) 1.1

Spl. % Aspal % Aspal Berat Berat Berat Berat B.J Persentase % Rongga % Rongga Marshall Stability Marshall
terhadap terhadap di di dalam kondisi Volume isi max. Rongga terhadap terisi Pembacaan Nilai Nilai Stabilitas Flow Quotient
No. Campuran Aggregate udara air SSD camp. di antara campuran aspal arloji stabilitas Setelah koreksi
% % gr gr gr cc gr / cc gr / cc aggregate % % mm kg kg mm kg / mm
E-D C/F 100-(100-b),G
100-(100G/H) 100-(I-J) O/P
V
A B C D E F G H I J K M N O P Q
1 5.25 5.54 1256 734 1268 534 2.351 88 1232 1183 3.4 347.9
2 1242 723 1272 549 2.263 81 1134 1089 3.0 362.9
3 1256 733 1265 532 2.361 83 1162 1116 3.3 338.0
Avg 5.25 5.54 538.333 2.325 3.824 42.9 39.2 17.8 1129 3.2 349.6
PERENDAMAN 24 JAM PADA SUHU 60°C
1 5.25 5.54 1241 722 1273 551 2.252 79 1106 1062 2.7 393.2
2 1251 728 1262 534 2.343 81 1134 1089 3.0 362.9
3 1267 741 1275 534 2.372 72 1008 968 2.5 387.1
Avg 5.25 5.54 539.667 2.323 3.824 43.0 39.3 17.7 1039 2.7 381.1

STABILITAS SISA SETELAH PERENDAMAN 24 JAM PADA SUHU 60°C Min. 85% = 1039 / 1129 x 100 = 92.1 %
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

DATA KALIBRASI BUKAAN COLDBIN

PARIASI AGGREGATE
No. MATERIAL BUKAAN COLD WAKTU KADAR
BIN BRT. BASAH BRT. KERING
AIR
( cm ) ( detik ) ( kg ) (%) ( kg )
4 10 19.4 8.7% 17.5
I COARSE AGGREGATE 6 10 56.7 8.7% 51.3
8 10 93.7 8.7% 84.7
4 10 32.7 9.7% 30.1
II MEDIUM AGGREGATE 6 10 49.8 9.7% 45.8
8 10 69.0 9.7% 63.4
4 10 15.7 4.8% 14.9
III DUST STONE 6 10 39.5 4.8% 37.6
8 10 62.8 4.8% 59.8
4 10 9.7 7.4% 9.4
IV SAND 6 10 19.7 7.4% 19.0
8 10 29.7 7.4% 28.6

Kapasitas Produksi AMP = 800 kg/menit


Kadar Aspal = 5.25 %
Berat Aggregat Kering = 758 kg/menit

Komposisi Agregat :

COARSE AGGREGATE = 20 % x 758 = 151.6 kg/menit = 25.3 kg/10 detik


MEDIUM AGGREGATE = 40 % x 758 = 303.2 kg/menit = 50.5 kg/10 detik
DUST STONE = 25 % x 758 = 189.5 kg/menit = 31.6 kg/10 detik
SAND = 15 % x 758 = 113.7 kg/menit = 19.0 kg/10 detik

Bukaan Cold Bin : 10000%

Cold Bin I = 4.4 cm


Cold Bin II = 7.2 cm
Cold Bin III = 5.4 cm
Cold Bin IV = 6.1 cm
LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

DATA KALIBRASI BUKAAN COLDBIN

COARSE AGG. = 40 % x 759 = 303.6 kg/menit = 50.6 kg/10 detik


BER AT MAT ER IAL (kg/ 10 detik)

GRAFIK BUKAAN

70

50.6 kg
60

50

40
7,2 cm

30

20

10

0
4 6 8

BUKAAN COLDBIN (cm)


LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC
NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

DATA KALIBRASI BUKAAN COLDBIN

COARSE AGG. = 20 % x 759 = 151.8 kg/menit = 25.3 kg/10 detik


BER AT MAT ER IAL (kg/ 10 detik)

GRAFIK BUKAAN

90

80

70

60

50

40
25,3 kg
30

20
4,4 cm

10

0
4 6 8

BUKAAN COLDBIN (cm)


LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC

NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

DATA KALIBRASI BUKAAN COLDBIN

COARSE AGG. = 25 % x 759 = 189.8 kg/menit = 31.6 kg/10 detik


BER AT MAT ER IAL (kg/ 10 detik)

GRAFIK BUKAAN

70

60

50

40 31,6 kg

30
5,4 cm

20

10

0
4 6 8

BUKAAN COLDBIN (cm)


LABORATORIUM JALAN RAYA
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - BC

NAMA PAKET :
LOKASI :
KONTRAKTOR :
KONSTRUKSI :

DATA KALIBRASI BUKAAN COLDBIN

COARSE AGG. = 15 % x 759 = 113.9 kg/menit = 19.0 kg/10 detik


BER AT MAT ER IAL (kg/ 10 detik)

GRAFIK BUKAAN

35

30

25
19.0 kg

20
6.1 cm

15

10

0
4 6 8

BUKAAN COLDBIN (cm)


Lampiran tabel 1.10 Pengujian Titik Lembek Aspal
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PENGUJIAN TITIK LEMBEK ASPAL


LOKASI : LABORATORIUM ASPAL
TANGGAL/HARI : 07 NOVEMBER 2018 / RABU
KELAS : DIV - 3D
KELOMPOK :2

Suhu yang Waktu Titik Lembek (˚C)


No. diamati (˚C) 1 2 Kanan Kiri
1 0 0 0
2 5 2'09" 2'09"
3 10 3'13" 3'13"
4 15 3'52" 3'52"
5 20 6'58" 6'58"
6 25 9'52" 9'52"
51˚ 53˚
7 30 11'52" 11'52"
8 35 12'57" 12'57"
9 40 14'20" 14'20"
10 45 16'18" 16'18"
11 50 17'54" 17'54"
51˚ 53˚
Rata- rata titik lembek (˚C)
52˚
Lampiran Tabel 1.11 Pengujian Penetrasi Aspal
JURUSAN TEKNIK SIPIL
POLITEKNIK NEGERI LHOKSEUMAWE
MIX DESING LASTON AC - WC

NAMA KEGIATAN : PENGUJIAN PENETRASI ASPAL


LOKASI : LABORATORIUM ASPAL
TANGGAL/HARI : 07 NOVEMBER 2018 / RABU
KELAS : DIV - 3D
KELOMPOK :2

Hasil Penetrasi
No. Sampel I
Penetrasi pada pengamatan ke 1 54
Penetrasi pada pengamatan ke 2 99
Penetrasi pada pengamatan ke 3 78
Penetrasi pada pengamatan ke 4 46
Penetrasi pada pengamatan ke 5 82
Rata-rata penetrasi 71.8
Total rata-rata penetrasi 71.8

Catatan : Besarnya nilai penetrasi yang disyaratkan yaitu 50 - 149


Lampiran Tabel 1.14 Tabel Angka Koreksi
TABEL ANGKA KOREKSI

KADAR TEBAL 1 TEBAL 2 TEBAL 3 TEBAL RATA-RATA DIAMETER DIAMETER DIAMETER RATA- VOLUME ANGKA
NO
KOREKSI PB (mm) (mm) (mm) (mm) 1 (mm) 2 (mm) RATA (mm) (cmᶟ) KOREKSI
5.00 1 6.60 6.65 6.63 6.63 10.21 10.22 10.21 542.27 0.91
2 6.67 6.62 6.73 6.67 10.25 10.18 10.21 546.09 0.89
3 6.81 6.90 6.81 6.84 10.22 10.25 10.23 562.20 0.86

KADAR TEBAL 1 TEBAL 2 TEBAL 3 TEBAL RATA-RATA DIAMETER DIAMETER DIAMETER RATA- VOLUME ANGKA
NO
KOREKSI PB (mm) (mm) (mm) (mm) 1 (mm) 2 (mm) RARA (mm) (cmᶟ) KOREKSI
5.50 1 6.56 6.67 6.56 6.60 10.20 10.33 10.27 545.65 0.89
2 6.62 6.56 6.56 6.58 10.24 10.25 10.25 542.15 0.91
3 6.78 6.66 6.63 6.69 10.25 10.26 10.25 552.02 0.88

KADAR TEBAL 1 TEBAL 2 TEBAL 3 TEBAL RATA-RATA DIAMETER DIAMETER DIAMETER RATA- VOLUME ANGKA
NO
KOREKSI PB (mm) (mm) (mm) (mm) 1 (mm) 2 (mm) RARA (mm) (cmᶟ) KOREKSI
6.00 1 6.62 6.63 6.67 6.64 10.26 10.26 10.26 548.43 0.89
2 6.55 6.45 6.45 6.48 10.28 10.28 10.28 537.58 0.92
3 6.52 6.43 6.49 6.48 10.24 10.21 10.22 531.57 0.94
KADAR
TEBAL 1 TEBAL 2 TEBAL 3 TEBAL RATA-RATA DIAMETER 1 DIAMETER 2
KOREKSI NO
(mm) (mm) (mm) (mm) (mm) (mm)
PB
5.50 1 6.56 6.67 6.56 6.60 10.20 10.33
2 6.62 6.56 6.56 6.58 10.24 10.25
3 6.78 6.66 6.63 6.69 10.25 10.26
DIAMETER RATA-RARA VOLUME ANGKA
(mm) (cmᶟ) KOREKSI
10.27 545.65
10.25 542.15
10.25 552.02
KADAR KADAR KADAR KADAR KADAR
KADAR KADAR
KOREKSI KOREKSI KOREKSI KOREKSI KOREKSI KADAR KOREKSI PB
KOREKSI PB KOREKSI PB
PB PB PB PB PB
6.00 1 6.62 6.63 6.67 6.64 10.26 10.26
2 6.55 6.45 6.45 6.48 10.28 10.28
3 6.52 6.43 6.49 6.48 10.24 10.21
KADAR KADAR
KADAR KOREKSI PB KOREKSI KOREKSI
PB PB
10.26 548.43
10.28 537.58
10.22 531.57

Anda mungkin juga menyukai